Electrochromic energy storage device using graphite foil counter electrode and application of electrochromic energy storage device

By using graphite foil as the electrode of the electrochromic device, matching the tungsten oxide negative electrode and using Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte, the low power density and oxidation of zinc-based electrochromic energy storage devices are solved. The problem of low tungsten redox potential achieves high energy density and stability, and enhances the application value of tungsten oxide electrochromic batteries.

CN118919902APending Publication Date: 2024-11-08HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148033.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing zinc-based electrochromic energy storage devices have low power density and low redox potential of tungsten oxide, which leads to poor effect of tungsten oxide electrochromic batteries as positive electrodes in the whole battery, limiting their application value.

Method used

Graphite foil is used as the electrode of the electrochromic device, matches the negative electrode of tungsten oxide to form a new electrochromic battery system. Graphite foil is used as the positive electrode to increase the discharge voltage, and uses Zn(OTF)2-Al(OTF)3 salt-in-water electrolysis. to increase energy density.

Benefits of technology

Significantly improves the discharge platform and energy density of tungsten oxide-based electrochromic batteries, achieves high optical modulation capability, fast response time and excellent cycling stability, and the universality and safety of graphite foils improve electrochromic devices. overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919902A_ABST
    Figure CN118919902A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochromic energy storage device using a graphite foil counter electrode and application of the electrochromic energy storage device. The electrochromic energy storage device comprises an ion storage layer, an electrolyte layer and an electrochromic layer which are stacked in sequence. The ion storage layer is graphite foil, and the electrochromic layer is tungsten oxide. The graphite foil better matched with the electrochromic layer WO3 is selected as the counter electrode, an effective voltage platform is remarkably improved, the graphite foil counter electrode can be matched with single or multiple cationic electrolytes, and the universality of the electrolytes is improved. The electrochromic energy storage device can realize neutral color modulation in a visible light range, is high in modulation rate, and is high in modulation rate retention rate before and after 5000 cycles. Under the condition of no voltage driving, the modulation rate attenuation of the electrochromic energy storage device is reduced after the electrochromic energy storage device is placed for 24 hours, and the electrochromic energy storage device has high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrochromic energy storage device, in particular to an electrochromic energy storage device in which metal counter electrodes zinc and aluminum of current electrochromic energy storage devices are replaced by graphite foil, and also to the application of the electrochromic energy storage device, belonging to the technical field of electrochromic devices. Background Art

[0002] Electrochromic energy storage devices (EESDs) can also be called electrochromic batteries. They are usually composed of a "sandwich" structure, including an electrochromic electrode, an electrolyte layer, and an ion storage layer. The electrolyte acts as an ion conduction medium between the electrochromic material and the ion storage layer, which promotes effective ion transfer and thus achieves reversible color change. 3+ The trivalence and small ionic radius (0.53 A˚) of Al 3+ Cations as charge carriers can bring fast switching speed, high optical contrast and high stability to WO3 electrochromic electrodes; using Zn 2+ and Al 3+ The mixed cation electrolyte composed of zinc or aluminum salts is conducive to the construction of electrochromic devices with high stability and high optical contrast. Generally, when zinc salts or aluminum salts are used as electrolytes, the paired electrodes should be zinc or aluminum metal electrodes. This is because the properties of zinc or aluminum salt electrolytes match the activity of zinc or aluminum electrodes, and can remain stable during the electrolysis process to provide the required current and voltage output. This combination not only takes into account the activity of the metal, but also the chemical stability of the electrolyte to ensure the performance and safety of the battery. However, electrochromic batteries constructed using metal zinc and aluminum as negative electrodes and tungsten oxide positive electrodes have more serious defects, which hinder the use of tungsten oxide electrochromic batteries.

[0003] Zhao et al., Trace H2O2-Assisted High-Capacity Tungsten Oxide Electrochromic Batteries with Ultrafast Charging in Seconds, AngewandteChemie International Edition, 56(51): 16111-16111, described that a tungsten oxide-Al electrochromic battery was constructed by using a tungsten oxide film as the positive electrode, an aluminum sheet as the negative electrode, and AlCl3 as the electrolyte, thus achieving a unified combination of optical regulation and energy storage. 3+ The redox potential of H + It is difficult to convert Al into 3+Therefore, during the coloring / fading (i.e., charging / discharging) cycle, the Al electrode is continuously oxidized and consumed, resulting in a high polarization rate and a short lifespan.

[0004] 《Li et al., Rechargeable Aqueous Hybrid Zn 2+ / Al 3+ ElectrochromicBatteries, Joule, 2019, 9(3), 2268-2278, Li et al. proposed to use a Zn negative electrode with low redox potential (-0.76 V vs. SHE) and good water stability to construct a tungsten oxide-Zn electrochromic battery. 2+ The poor kinetic performance of cationic electrolytes will limit the capacity, switching speed and optical contrast of tungsten oxide-Zn electrochromic batteries, hindering the use of tungsten oxide electrochromic batteries. At the same time, during the discharge process, due to the reduction of tungsten oxide, the discharge voltage drops rapidly, and the discharge platform of tungsten oxide-Zn electrochromic batteries is around 0.2 V, resulting in low power density and low practical application value. Summary of the invention

[0005] In view of the low power density of zinc-based electrochromic energy storage devices, which are currently widely studied, and the redox potential (Φ(W 6+ / W 5+ The present invention provides an electrochromic energy storage device using a graphite foil counter electrode. The electrochromic energy storage device uses a graphite foil with a high redox potential as a counter electrode and matches a tungsten oxide negative electrode to construct a new electrochromic battery system, which is expected to improve the discharge platform of tungsten oxide-based electrochromic batteries and significantly increase the energy density.

[0006] The specific technical solutions of the present invention are as follows: An electrochromic energy storage device, also known as an electrochromic battery, includes an ion storage layer, an electrolyte layer and an electrochromic layer stacked in sequence; the ion storage layer is graphite foil, and the electrochromic layer is tungsten oxide. The electrochromic layer, the electrolyte layer and the ion storage layer form a sandwich structure, and a certain sealed space is formed between the electrochromic layer and the ion storage layer for injecting the electrolyte layer.

[0007] Furthermore, the graphite foil of the present invention is used as the positive electrode and tungsten oxide is used as the negative electrode, which improves the discharge voltage of the electrochromic energy storage device. The graphite foil will not cause structural damage due to the use of the aqueous electrolyte layer. At the same time, the graphite foil is a direct commercial product with uniform product thickness and material, good controllability, and can be simply compounded with the base layer through an adhesive. Compared with powdered graphite that needs to be attached to the base layer by brushing, it is easy to operate and has strong controllability of electrode quality.

[0008] Furthermore, the graphite foil is preferably in the form of a graphite foil frame with a hollow center, which can improve the light transmittance of the electrochromic device.

[0009] Furthermore, the thickness of the graphite foil is 0.1-0.5 mm, such as 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, and 0.5 mm, and the thickness of the graphite foil has no significant effect on the performance. The present invention selects graphite foil as the ion storage layer, that is, the counter electrode. Graphite foil can replace the metal counter electrodes zinc and aluminum of the current electrochromic energy storage device, and can also achieve independent regulation to achieve color overlap to achieve high modulation rate without considering charge matching. In addition, graphite foil has fast ion adsorption / desorption kinetics, excellent conductivity and good stability. The electrochromic energy storage device manufactured using graphite foil has high optical modulation capability, fast response time and excellent cycle stability.

[0010] Furthermore, the present invention selects graphite foil as the counter electrode. Unlike the zinc counter electrode system which must have zinc ions as the main or supporting electrolyte, graphite foil as the counter electrode can match a single or multiple cationic electrolytes (such as NH4 + ,K + , Li + , Zn 2+ / Al 3+ etc.), which is universal.

[0011] Preferably, the electrolyte layer of the present invention is an aqueous electrolyte, and the aqueous electrolyte is a Zn(OTF)2-Al(OTF)3 water-in-salt (WiSE) electrolyte, which is safer and more environmentally friendly and has the advantages of a wide voltage window and multivalent metal ion conversion.

[0012] Furthermore, the Zn(OTF)2-Al(OTF)3 water-in-salt (WiSE) electrolyte is composed of Zn(OTF)2, Al(OTF)3 and water. In the water-in-salt electrolyte, the concentration of Zn(OTF)2 is 3m, and the concentration of Al(OTF)3 is 1m, where the unit m is the concentration unit, which represents the ratio of the molar amount of Zn(OTF)2 or Al(OTF)3 to the volume of water, that is, the ratio of Zn(OTF)2 to water is 3mol:1L, and the ratio of Al(OTF)3 to water is 1mol:1L.

[0013] Preferably, the tungsten oxide is amorphous WO3, which can be obtained by magnetron sputtering.

[0014] Preferably, the thickness of the electrochromic layer is 390-410 nm, preferably 400 nm.

[0015] Furthermore, one side of the ion storage layer is in contact with the electrolyte layer, and the other side is connected to the first substrate layer; one side of the electrochromic layer is in contact with the electrolyte layer, and the other side is in contact with the conductive layer, and the conductive layer is connected to the second substrate layer.

[0016] Furthermore, the ion storage layer and the first substrate layer are fixed with butyl tape. The electrochromic layer is opposite to the ion storage layer, and the electrochromic layer and the ion storage layer are fixed with butyl tape and a certain space is encapsulated, and the aqueous electrolyte is filled in the space with a needle. The conductive layer and the second substrate layer are fixed with butyl tape.

[0017] Furthermore, the electrochromic energy storage device includes a first substrate layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a conductive layer, and a second substrate layer stacked in sequence.

[0018] Furthermore, the material of the conductive layer is selected from FTO and ITO.

[0019] Furthermore, the materials of the first substrate layer and the second substrate layer are independently selected from glass, plastic, etc.

[0020] Furthermore, the preparation and assembly method of the electrochromic energy storage device of the present invention can be carried out by referring to the preparation method of the electrochromic energy storage device in the prior art, which is not difficult for those skilled in the art.

[0021] In a specific embodiment of the present invention, a method for preparing an electrochromic energy storage device is provided, comprising the following steps: 1. Forming an electrochromic layer on the conductive layer by magnetron sputtering; 2. Dissolve Zn(OTF)2 and Al(OTF)3 in water to prepare a water-in-salt (WiSE) electrolyte; 3. The first substrate layer, the ion storage layer, the electrochromic layer, the conductive layer, and the second substrate layer are stacked and packaged in sequence, and then an electrolyte layer is injected between the ion storage layer and the electrochromic layer to obtain an electrochromic energy storage device.

[0022] Furthermore, the present invention also provides an application of graphite foil as an ion storage layer of an electrochromic device or an electrochromic energy storage device.

[0023] Furthermore, the present invention also provides a use of a Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte as an electrolyte layer of an electrochromic device or an electrochromic energy storage device. The definition of the Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte is consistent with the above description.

[0024] The present invention has the following beneficial effects: 1. The present invention selects graphite foil that is more compatible with the electrochromic layer WO3 as the counter electrode. The graphite foil has excellent ductility and can be independently regulated to achieve color overlap and high modulation rate without considering charge matching, thereby significantly improving the effective voltage platform.

[0025] 2. The graphite foil of the present invention has fast ion adsorption / desorption kinetics, excellent conductivity and good stability. The electrochromic energy storage device manufactured using the graphite foil has high optical modulation capability, fast response time and excellent cycle stability.

[0026] 3. The graphite foil of the present invention is used as the positive electrode and tungsten oxide is used as the negative electrode, which improves the discharge voltage of the electrochromic energy storage device. 4. The present invention selects graphite foil with high redox potential as the counter electrode, which can be matched with single or multiple cationic electrolytes (such as NH4 + ,K + , Li + , Zn 2+ / Al 3+ The present invention preferably uses Zn(OTF)2- Al(OTF)3 salt-in-water electrolyte as the electrolyte layer, which can provide a voltage range of up to 1.8 V and significantly improve the energy density.

[0027] 5. The electrochromic energy storage device of the present invention can achieve neutral color modulation in the visible light range, with a modulation rate as high as 80.9%, and the modulation rate retention rate is 97.68% before and after 8000 cycles.

[0028] 6. When the electrochromic energy storage device of the present invention is placed without voltage drive, the modulation rate only decays by 1.87% after 24 hours, and has high stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the structure of the electrochromic energy storage device of the present invention, wherein: 1. a first substrate layer; 2. an ion storage layer; 3. an electrolyte layer; 4. an electrochromic layer; 5. a conductive layer; and 6. a second substrate layer.

[0030] Figure 2 The electrochromic energy storage device of Example 1 of the present invention is 0.5 mA / cm 2 GCD curves at different current densities.

[0031] Figure 3 The electrochromic energy storage device of Comparative Example 1 is 0.5 mA / cm 2 GCD curves at different current densities.

[0032] Figure 4 The figure shows the rate performance of the electrochromic energy storage device of Example 1 of the present invention at different current densities.

[0033] Figure 5 The figure shows the rate performance of the electrochromic energy storage device of comparative example 1 at different current densities.

[0034] Figure 6 This is a comparison chart of the energy densities of the GF / / WO3 electrochromic energy storage device of the present invention and the WO3 / / Zn electrochromic energy storage device of comparative example 1.

[0035] Figure 7 This is a graph of the optical stability of the electrochromic energy storage device of Example 1 of the present invention recorded at a wavelength of 700 nm for 8000 cycles (coloring at 1.8 V for 30 s, fading at 0 V for 60 s).

[0036] Figure 8 This is a graph of the optical stability of the WO3 / / Zn electrochromic energy storage device of Comparative Example 1 after 100 cycles at a wavelength of 700 nm (coloring at 0.1 V for 30 s, fading at 1.2 V for 60 s).

[0037] Fig. 9 The GF / / WO3 electrochromic energy storage device of Example 1 of the present invention is colored at 1.8 V for 30 s, and the WO3 / / Zn electrochromic energy storage device of Comparative Example 1 is colored at 0.1 V for 30 s, and then the optical transmittance of the electrochromic energy storage device is monitored at a wavelength of 700 nm under open circuit conditions. DETAILED DESCRIPTION

[0038] The following is a description of exemplary embodiments of the present invention, including various details of the embodiments of the present invention to aid understanding, which should be considered as merely exemplary. Therefore, it should be appreciated by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present invention. Likewise, for clarity and simplicity, descriptions of well-known functions and structures are omitted in the following description.

[0039] Unless otherwise defined, the technical and scientific terms in this specification have the same meaning as those commonly understood by those skilled in the art. Although similar or identical methods and materials as those described herein may be used in experiments or practical applications, the present invention still describes the materials and methods below. In the event of a conflict, the present specification, including definitions, shall prevail.

[0040] Example 1 An electrochromic energy storage device comprises a first substrate layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a conductive layer, and a second substrate layer stacked in sequence, wherein the first substrate layer and the second substrate layer are transparent glass, the conductive layer is FTO, the ion storage layer is a graphite foil frame, the electrochromic layer is amorphous WO3, and the electrolyte layer is a 3 m Zn(OTF)2-1 m Al(OTF)3 salt-in-water (WiSE) electrolyte. The graphite foil frame is a directly commercially available graphite foil in a hollow rectangular shape, and its size and shape match those of the first substrate layer. The width of the graphite foil in the graphite foil frame is 0.3 cm, and the thickness of the graphite foil is 0.5 mm.

[0041] The preparation method of the electrochromic device is as follows: 1. Preparation of electrochromic layer WO3 sample: Under the conditions of power of 100 W, DC sputtering pressure of 1.5 Pa, Ar:O2=3:1 (volume ratio), and sputtering time of 30 min, magnetron sputtering was performed using a tungsten target to obtain amorphous WO3 on FTO with a thickness of about 400 nm.

[0042] 2. Preparation of 3 m Zn(OTF)2-1 m Al(OTF)3 salt-in-water (WiSE) electrolyte: 21.81 g Zn(OTF)2 and 9.48 g Al(OTF)3 were dissolved in 20 g deionized water to prepare a 3 m Zn(OTF)2-1 m Al(OTF)3 salt-in-water (WiSE) electrolyte.

[0043] 3. Use WO3 and graphite foil (GF) to construct an electrochromic energy storage device: The electrochromic energy storage device consists of WO3 loaded on FTO, a graphite foil frame, bare glass and 3 m Zn(OTF)2-1 m Al(OTF)3WiSE. WO3 acts as the electrochromic layer, the graphite foil acts as the ion storage layer, and the bare glass acts as the encapsulation layer. The detailed assembly process is: first, cover WO3 / FTO with a butyl tape with a width of 0.5 cm and a thickness of 1 mm, and then cover the graphite foil frame on WO3 / FTO. Cover the bare glass with a butyl tape with a width of 0.5 cm and a thickness of 0.5 mm, and then cover the bare glass on the graphite foil frame on the other side and the FTO on the other side respectively. Use a syringe to inject electrolyte into the remaining space between the graphite foil frame and WO3 to form a Figure 1 Electrochromic energy storage device with the structure shown.

[0044] Comparative Example 1 1. Preparation of electrochromic layer WO3 sample: same as in Example 1.

[0045] 2. Preparation of 3 m Zn(OTF)2-1 m Al(OTF)3 water-in-salt (WiSE) electrolyte: same as Example 1.

[0046] 3. Construct an electrochromic energy storage device using WO3 and zinc foil (Zn): The electrochromic energy storage device consists of WO3 loaded on FTO, zinc foil frame, bare glass and 3 m Zn(OTF)2-1 m Al(OTF)3WiSE, and the zinc foil frame is 0.3 cm wide and 0.5 mm thick. WO3 acts as an electrochromic layer, zinc foil acts as an ion storage layer, and bare glass acts as an encapsulation layer. The detailed assembly process is as follows: first, a butyl tape with a width of 0.5 cm and a thickness of 1 mm is covered on WO3 / FTO, and then the zinc foil frame is covered on WO3 / FTO. The bare glass is covered with a butyl tape with a width of 0.5 cm and a thickness of 0.5 mm, and then the bare glass is covered on the zinc foil frame on the other side and the FTO on the other side. The electrolyte is injected into the remaining space between the zinc foil frame and WO3 with a syringe to form a WO3 / / Zn electrochromic energy storage device.

[0047] Performance Verification 1. Charge and discharge performance test 1.1 Experimental method: The rate performance of the electrochromic energy storage device (EESD) assembled in Example 1 and Comparative Example 1 was tested using a Xinwei battery tester, with the current density set to 0.5 mA / cm 2 , repeat 3 times.

[0048] The experimental results of Example 1 are as follows Figure 2 As shown in the figure, it can be seen that the current density is 0.5 mA / cm2 When the capacity of Example 1 is 327.6 mAh / m 2 , which shows that Example 1 has a stable high discharge capacity.

[0049] The experimental results of Comparative Example 1 are as follows Figure 3 As shown in the figure, it can be seen that the current density is 0.5 mA / cm 2 When the capacity of Example 1 is 43.6 mAh / m 2 , the results show that the discharge capacity of Comparative Example 1 is lower.

[0050] 2. Rate performance test 2.1 Experimental method: The rate performance of the electrochromic energy storage device (EESD) assembled in Example 1 and Comparative Example 1 was tested using a Xinwei battery tester, with the current density set to 0.3 mA / cm 2 , 0.4 mA / cm 2 , 0.5 mA / cm 2 , 0.6 mA / cm 2 , 0.7 mA / cm 2 , and each current density was cycled 3 times.

[0051] The experimental results of Example 1 are as follows Figure 4 As shown in the figure, it can be seen that the current density is 0.3-0.7 mA / cm 2 When 419.2 mAh / m 2 , 360.0 mAh / m 2 , 327.6 mAh / m 2 , 300.0 mAh / m 2 , 275.2 mAh / m 2 The high capacity of 2 GF / / WO3 can still recover 388.4mAh / m 2 This shows that Example 1 has good rate stability.

[0052] The experimental results of Comparative Example 1 are as follows Figure 5 As shown in the figure, it can be seen that the current density is 0.3-0.7 mA / cm 2 When , Example 1 can obtain 64.8 mAh / m 2 , 50.8 mAh / m 2 , 40.4 mAh / m 2 , 33.2 mAh / m 2 , 27.2 mAh / m 2The capacity of 2 WO3 / / Zn can still recover 59.2 mAh / m 2 The reversible capacity of Comparative Example 1 is shown to be good in reversibility, but the capacity is relatively low.

[0053] 3. Energy density and power density performance test Experimental method: The rate performance of the EESD assembled in Example 1 and Comparative Example 1 was tested using a Xinwei battery tester, with the current density set to 0.3 mA / cm 2 , 0.4 mA / cm 2 , 0.5 mA / cm 2 , 0.6 mA / cm 2 , 0.7 mA / cm 2 , and each current density was cycled 3 times.

[0054] The experimental results are as follows Figure 6 As shown in the figure, it can be seen that under the same power density, the energy density of the new GF / / WO3 can reach ten times that of WO3 / / Zn.

[0055] 3. Spectral cycle performance 3.1 Experimental method: The electrochromic energy storage device (EESD) assembled in Example 1 was subjected to in-situ spectral cycling performance test at a wavelength of 700 nm by means of electrochemical and optical coupling. The electrochemical workstation selected the STEP-Multi-Potential-Steps test program, set the first step program to 1.8 V, 30 s, the second step program to 0 V, 60 s, and the number of cycles was set to 8000.

[0056] The experimental results are as follows Figure 7 As shown in the figure, it can be seen that the modulation rate at a wavelength of 700 nm is 80.9%, and after 8000 dyeing / bleaching cycles, the optical modulation rate of the device is still 97.7% of the initial value, with high stability.

[0057] 3.2 Experimental method: The electrochromic energy storage device (EESD) assembled in Comparative Example 1 was subjected to in-situ spectral cycling performance test at a wavelength of 700 nm by means of electrochemical and optical coupling. The electrochemical workstation selected the STEP-Multi-Potential-Steps test program, set the first step to 0.1 V, 30 s, the second step to 1.2 V, 60 s, and the number of cycles to 100.

[0058] The experimental results are as follows Figure 8As shown in the figure, it can be seen that the modulation rate at a wavelength of 700 nm is 81.7%, but after 60 dyeing / bleaching cycles, the optical modulation rate of the device drops sharply and the stability is poor.

[0059] 4. Static stability performance Experimental method: The spectrometer selects time scanning, sets the wavelength to 700 nm, the scanning time to 86400 s, and uses air as the baseline. The electrochemical workstation selects the it-Amperometric it Curve test program, sets 1.8 V, 30 s to color the electrochromic energy storage device (EESD) assembled in Example 1. Set 0.1 V, 30 s to color the electrochromic energy storage device (EESD) assembled in Comparative Example 1. After coloring, the transmittance is monitored for 24 hours using a spectrometer without applying voltage.

[0060] The experimental results are as follows Fig. 9 As shown in the figure, it can be seen that the modulation rate of the device assembled in Example 1 only decays by 1.87% after being placed for 24 hours, while the modulation rate of the comparative example 1 decays by 45.3% after being placed for 24 hours, which indicates that the device assembled in Example 1 has excellent optical stability.

Claims

1. An electrochromic energy storage device, characterized in that: The electrochromic energy storage device comprises an ion storage layer, an electrolyte layer and an electrochromic layer which are stacked in sequence; the ion storage layer is graphite foil, and the electrochromic layer is tungsten oxide.

2. The electrochromic energy storage device according to claim 1, characterized in that: The graphite foil is in a hollow frame shape.

3. The electrochromic energy storage device according to claim 1, characterized in that: The graphite foil has a thickness of 0.1-0.5 mm.

4. The electrochromic energy storage device according to any one of claims 1 to 3, characterized in that: The electrolyte layer is a Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte; preferably, the Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte is composed of Zn(OTF)2, Al(OTF)3 and water.

5. The electrochromic energy storage device according to claim 4, characterized in that: The ratio of Zn(OTF)2 to water in the electrolyte is 3 mol:1L, and the ratio of Al(OTF)3 to water is 1 mol:1L.

6. The electrochromic energy storage device according to any one of claims 1 to 5, characterized in that: The tungsten oxide is amorphous WO3.

7. The electrochromic device according to any one of claims 1 to 5, characterized in that: One side of the ion storage layer is in contact with the electrolyte layer, and the other side is connected to the first substrate layer; one side of the electronic color-changing layer is in contact with the electrolyte layer, and the other side is in contact with the conductive layer, and the conductive layer is connected to the second substrate layer.

8. The electrochromic device according to claim 7, characterized in that: The material of the conductive layer is selected from FTO and ITO; preferably, the materials of the first substrate layer and the second substrate layer are independently selected from glass and plastic.

9. Application of graphite foil as an ion storage layer of an electrochromic device or an electrochromic energy storage device.

10. Application of Zn(OTF)2-Al(OTF)3 salt-in-water electrolyte as the electrolyte layer of electrochromic devices or electrochromic energy storage devices.