Circuit board manufacturing method and circuit board
By controlling the current density of gold plating and subsequent process optimization, the problem of nickel gold layer lifting and falling off during the oblique edge of gold plating finger on the circuit board is solved, reducing the risk of short circuit, ensuring the stability of nickel gold layer and the electroplating layer Uniformity.
Patent Information
- Application Number
- CN202410902729.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the circuit board is prone to rising and falling off during the oblique edge of the gold finger, resulting in an increase in the risk of short circuit.
By controlling the current density during electroplating of gold in the range of 0.6ASD≤J≤0.8ASD, and the oblique edges are performed after the substrate is formed, combining the optimization of baking sheet, brightener concentration and tool life, the interior of the nickel gold layer is reduced. Stress and brittleness to prevent the nickel-gold layer from rising and falling off.
It effectively reduces the risk of short circuit on the circuit board, ensures the stability of the nickel-gold layer and the uniformity of the electroplating layer, and avoids the problem of the nickel-gold layer rising and falling off after the oblique edge.
Smart Images

Figure CN118921884A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of circuit boards, and more specifically, to a circuit board manufacturing method and a circuit board. Background Art
[0002] When the gold finger of the circuit board needs to be electroplated, it is usually necessary to design a gold finger guide wire so that the gold finger can be electroplated by energizing the gold finger guide wire. After the electroplating of the gold finger is completed, the gold finger guide wire needs to be removed.
[0003] In the related art, the gold finger is usually beveled to remove the lead, but the bevel is likely to cause the gold finger lead to lift up or fall off. The fallen nickel-gold layer can easily enter the welding surface, increasing the risk of short circuit on the circuit board. Summary of the invention
[0004] The purpose of the embodiments of the present application is to provide a circuit board manufacturing method and a circuit board to solve the technical problem of increased short circuit risk of the circuit board in the prior art.
[0005] To achieve the above purpose, the technical solution adopted in this application is:
[0006] In a first aspect, a circuit board manufacturing method is provided, the method comprising:
[0007] Providing a substrate, the substrate having a gold finger;
[0008] The gold finger is electroplated with gold, wherein the current density of the electroplated gold is J, and the value range of J is: 0.6ASD≤J≤0.8ASD;
[0009] The gold fingers are beveled after the substrate is formed.
[0010] In the circuit board manufacturing method provided in the embodiment of the present application, the gold finger is electroplated with gold before the gold finger is beveled, and the current density J during the electroplating satisfies: 0.6ASD≤J≤0.8ASD. In this way, when the current density J is within the above value range, it is within the range of the available small current density. Within this range, as the current density increases, the polarization effect during the electroplating of gold is enhanced, the nucleation rate increases, the grains become finer, the corresponding porosity becomes smaller, and the stress becomes smaller, which is conducive to avoiding the problem of lead warping and falling off after beveling, and preventing the fallen nickel-gold layer from easily entering the welding surface, thereby reducing the risk of short circuit.
[0011] If J>0.8ASD, it is beyond the usable range. As the current density increases, the nucleation rate decreases, the lattice becomes coarser, and the stress increases, causing the lead to lift and fall off after the bevel. When J<0.6ASD, although the nucleation rate increases and the grain size decreases as the current increases, the stress cannot meet the requirements, and the lead still lifts and falls off after the bevel.
[0012] Therefore, the circuit board manufacturing method provided in the embodiment of the present application is conducive to avoiding the problem of lead curling and falling off after beveling, and preventing the fallen nickel-gold layer from easily entering the welding surface, thereby reducing the risk of short circuit in the circuit board.
[0013] In some embodiments, J is equal to 0.8ASD. At this current density, the electrochemical polarization effect is large, the cathode reaction overpotential is high, the critical radius of the crystal nucleus is reduced, the nucleation rate of the crystal is increased, and the nucleation rate of the crystal is greater than the growth rate. Therefore, when the current density J is equal to 0.8ASD, the nucleation rate reaches the highest, the grain size is the smallest, and the porosity is the smallest. At this time, the internal stress is in the optimal state, which is more conducive to avoiding the problem of lead warping and falling off after the bevel, thereby further reducing the risk of short circuit of the circuit board.
[0014] In some embodiments, after electroplating the gold finger and before beveling the gold finger after the substrate is formed, the circuit board manufacturing method provided by the present application further includes:
[0015] The substrate is baked, wherein the temperature of the baking plate is T, and the value range of T is: 150°C≤T≤180°C.
[0016] In this way, the circuit board manufacturing method provided by the present application can release the hydrogen evolution effect during gold electroplating, reduce the internal stress of the nickel layer, and improve the nickel brittleness problem of the nickel-gold layer, thereby helping to avoid the problem of lead warping and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0017] In some embodiments, after electroplating the gold finger and before beveling the gold finger after the substrate is formed, the circuit board manufacturing method provided by the present application further includes:
[0018] The substrate is baked, wherein the baking time is t, and the value range of t is: 60min≤t≤80min.
[0019] In this way, the circuit board manufacturing method provided by the present application can release the hydrogen evolution effect during gold electroplating, reduce the internal stress of the nickel layer, improve the nickel brittleness problem of the nickel-gold layer, and help avoid the problem of lead warping and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0020] In some implementations, when electroplating the gold finger, the concentration of the brightener in the electroplating solution is n, and the value range of n is: 0.1%≤n≤0.3%.
[0021] In this way, the circuit board manufacturing method provided by the present application controls the brightener concentration within a reasonable range, ensures the softness of the electroplated layer while enhancing the gloss and smoothness, and can also ensure the uniformity and stability of the plating layer, which can reduce the brittleness of the nickel layer and help avoid the problem of lead curling and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0022] In some embodiments, when the gold finger is beveled after the substrate is formed, the moving speed of the gold finger is v, and the value range of v is: 2m / min≤v≤3m / min.
[0023] In this way, the circuit board manufacturing method provided in the present application can reduce the travel speed and reduce the external force applied to the nickel-gold layer during beveling, thereby helping to avoid the problem of lead curling and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0024] In some implementations, when the gold finger is beveled after the substrate is formed, the life of the tool is L, and the value range of L is: 6m≤L≤8m.
[0025] In this way, the circuit board manufacturing method provided in the present application can reduce the life of the tool and reduce the external force applied to the nickel-gold layer during beveling, thereby helping to avoid the problem of lead warping and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0026] In some embodiments, the substrate also has a lead, which is connected to one end of the gold finger; before electroplating the gold finger with gold, the circuit board manufacturing method provided by the present application also includes: setting an anti-gold plating dry film on the substrate; wherein, when the anti-gold plating dry film is set on the substrate, a window is opened at the gold finger and at the part of the lead close to the gold finger.
[0027] In this way, the circuit board manufacturing method provided in the present application allows the lead wire portion close to the gold finger to be electroplated with gold, thereby avoiding the lead wire position not being electroplated with gold due to deviation of the bevel equipment.
[0028] In some embodiments, the window portion of the lead wire includes a first side and a second side opposite to each other, the first side is connected to the gold finger, the distance between the first side and the second side is d, and the value range of d is: 0.2mm≤d≤0.3mm.
[0029] In this way, the circuit board manufacturing method provided in the present application reserves a position for electroplating gold at the part of the lead close to the gold finger, thereby avoiding the lead position not being electroplated gold due to the deviation of the bevel equipment.
[0030] In a second aspect, the present application provides a circuit board, which is manufactured by the circuit board manufacturing method in the above embodiment. The circuit board provided by the present application has similar technical effects as the circuit board manufacturing method in the above embodiment, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0032] Figure 1 One of the partial structural schematic diagrams of the circuit board provided in the embodiment of the present application;
[0033] Figure 2 One of the structural schematic diagrams of the gold finger provided in the embodiment of the present application;
[0034] Figure 3 The second structural diagram of the gold finger provided in the embodiment of the present application;
[0035] Figure 4 The third structural diagram of the gold finger provided in the embodiment of the present application;
[0036] Figure 5 One of the schematic diagrams of the circuit board manufacturing method provided in the embodiment of the present application;
[0037] Figure 6 A schematic diagram of the inclined surface of the gold finger after gold plating at different current densities provided in the embodiment of the present application;
[0038] Figure 7 One of the schematic diagrams of the internal lattice of the gold finger after electroplating provided in the embodiment of the present application;
[0039] Figure 8 The second schematic diagram of the internal lattice of the gold finger after electroplating provided in the embodiment of the present application;
[0040] Fig. 9 A relationship diagram between the nucleation rate, grain size, porosity and current density of the gold finger provided in the embodiment of the present application after electroplating;
[0041] Fig.10 A data graph showing the nucleation rate, grain size, porosity, and current density of the gold finger after electroplating provided in an embodiment of the present application;
[0042] Fig.11A schematic diagram of the inclined surface of the gold finger provided in an embodiment of the present application after gold electroplating at different brightener concentrations;
[0043] Fig.12 A second schematic diagram of a method for manufacturing a circuit board provided in an embodiment of the present application;
[0044] Fig.13 The second schematic diagram of the partial structure of the circuit board provided in the embodiment of the present application;
[0045] Fig.14 for Fig.13 A partial enlarged view of point A in the middle;
[0046] Fig.15 This is a third schematic diagram of the circuit board manufacturing method provided in an embodiment of the present application.
[0047] Among them, the reference numerals in the figure are:
[0048] 1-gold finger; 101-grain; 102-pore; 11-slant; 12-dielectric layer; 13-copper layer; 14-nickel-gold layer; 141-nickel-gold dot; 15-notch; 2-lead; 21-unopened part; 22-opened part; m-first side; n-second side; 3-anti-gold plating dry film. DETAILED DESCRIPTION
[0049] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0050] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0051] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0052] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0053] See also Figure 1 When the gold finger 1 of the circuit board needs to be electroplated (nickel-gold layer), it is usually necessary to design a lead 2, which is connected to one end of the gold finger 1, so that the gold finger 1 can be electroplated by energizing the lead 2. After the electroplating of the gold finger 1 is completed, the lead 2 is not allowed to remain in the finished circuit board, and the lead 2 needs to be removed.
[0054] See also Figure 2 , especially for storage products, the lead 2 is designed at the front end of the gold finger 1, and the front end lead 2 is removed by beveling, that is, a bevel 11 is formed at the front end of the gold finger 1 after beveling. Usually, after the gold finger 1 is beveled, copper can be leaked at the bevel 11, but the problem of the nickel-gold layer 14 lifting and falling off after beveling is not allowed. The fallen nickel-gold layer 14 is easy to enter the welding surface, which will increase the risk of short circuit of the circuit board.
[0055] The inventors found that the main reason for the lifting and falling of the nickel-gold layer 14 is that when the nickel-gold layer 14 (mainly nickel layer, the gold layer is only thinner 0.05um and only plays a protective role) is subjected to external force on the bevel, if the nickel-gold layer 14 is brittle (nickel is brittle), cracks will appear in the nickel-gold layer 14 after the bevel. When the organic solderability preservatives (OSP) process is performed on the gold finger 1, the nickel-gold layer 14 is separated from the copper surface, resulting in the phenomenon of nickel-gold lifting and falling.
[0056] Please also read Figure 3 and Figure 4 The gold finger 1 includes an inner dielectric layer 12 and an outer copper layer 13, and the copper layer 13 wraps the dielectric layer 12. After electroplating, the nickel-gold layer 14 covers the copper layer 13, and the nickel-gold layer 14 is prone to form a nickel-gold point 141 with a crack at the edge of the inclined surface 11 of the gold finger 1, causing the nickel-gold point 141 to warp up or even fall off to form a gap 15.
[0057] Usually, in order to improve such defects, a selective film process is added to protect the gold surface and improve the problem of gold finger 1 lead 2 lifting and falling off after beveling. However, adding a selective film will increase the process and cost, and it is impossible to completely eliminate defects.
[0058] In order to solve the above technical problems, the embodiments of the present application provide a circuit board manufacturing method and a circuit board.
[0059] The inventors found that brittleness refers to the phenomenon that a material suddenly breaks without obvious deformation under the action of external force. The external force can be mechanical force or thermal stress caused by thermal expansion and contraction. One of the main factors causing nickel brittleness is internal stress. When the internal stress of the nickel-gold layer 14 is large, cracks will appear in the nickel-gold layer 14 when it is subjected to external force at an angle.
[0060] Since the stress of the plating layer is formed by the electroplating itself, rather than the additional stress caused by the application of external force, the stress is concentrated in the plating layer, so the stress of the electroplating layer is called "internal stress". If the stress is not eliminated after electroplating, the internal stress generated in the electroplating will always exist. The greater the internal stress, the greater the brittleness.
[0061] See also Figure 5 , the circuit board manufacturing method provided in the embodiment of the present application is now described. The circuit board manufacturing method provided in the present application comprises the following steps:
[0062] S1, provide a substrate, the substrate has a gold finger 1 and a lead 2.
[0063] In step S1, the pre-process is completed according to the normal process to form a substrate, and then the subsequent processes are carried out. The pre-process includes: cutting, inner layer circuit, automated optical inspection (AOI), pressing, drilling target, milling edge, drilling, filling holes, circuit, solder mask, etc.
[0064] S2, electroplating gold on the gold finger 1. The current density of the electroplating gold is J, and the value range of J is: 0.6ASD≤J≤0.8ASD.
[0065] S3, beveling the gold finger 1 after the substrate is formed.
[0066] In the circuit board manufacturing method provided in the embodiment of the present application, the gold finger 1 is electroplated with gold before the gold finger 1 is beveled, and the current density J during the electroplating satisfies: 0.6ASD≤J≤0.8ASD.
[0067] After the circuit board manufacturing method provided in the embodiment of the present application performs beveling on the gold finger 1, the subsequent processes are completed in sequence. The subsequent processes include: electrical testing, automatic visual inspection (AVI), field quality control (FQC), organic solderability preservatives (OSP), finished quality control (FQC), factory quality assurance (FQA), packaging, etc.
[0068] Please also read Figure 3 , Figure 4 and Figure 6 , Figure 6 Figure a is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating gold at a current density of 0.4ASD. Figure 6 Figure b is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating gold at a current density of 0.6ASD. Figure 6 Figure c is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating gold at a current density of 0.8ASD. Figure 6 Figure d in the middle is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating gold at a current density of 1.0ASD. Figure 6 Figure e is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating gold at a current density of 1.2ASD. Figure 6 It can be seen that the nickel-gold point 141 of the gold finger 1 has fallen off after the gold finger 1 was electroplated with gold at a current density of 0.4ASD, the nickel-gold point 141 of the gold finger 1 did not warp or fall off after the gold finger 1 was electroplated with gold at a current density of 0.6ASD, the nickel-gold point 141 of the gold finger 1 did not warp or fall off after the gold finger 1 was electroplated with gold at a current density of 0.8ASD, the nickel-gold point 141 of the gold finger 1 was warped and did not fall off after the gold finger 1 was electroplated with gold at a current density of 1.0ASD, and the nickel-gold point 141 of the gold finger 1 has fallen off after the gold finger 1 was electroplated with gold at a current density of 1.2ASD.
[0069] Please also read Figure 7 and Figure 8 , Figure 7 This is a schematic diagram of the internal lattice of the gold finger 1 after electroplating at a current density greater than 0.8ASD. Figure 8 FIG. 1 is a schematic diagram of the internal lattice of the gold finger 1 after electroplating when the current density is greater than or equal to 0.6ASD and less than or equal to 0.8ASD. Figure 6 , Figure 7 and Figure 8It can be seen that when the current density J satisfies 0.6ASD≤J≤0.8ASD, it is within the range of available small current density. Within this range, as the current density increases, the polarization effect during gold plating is enhanced, the nucleation rate increases, the grains 101 become finer, the pores 102 become smaller, and the corresponding porosity and stress become smaller, which is beneficial to avoid the problem of lead 2 warping and falling off after beveling, and prevent the fallen nickel-gold layer 14 from easily entering the welding surface, thereby reducing the risk of short circuit.
[0070] If J>0.8ASD, it is beyond the usable range. As the current density increases, the nucleation rate decreases, the lattice becomes coarser, and the stress increases, causing the problem of lead 2 lifting and falling off after the bevel. When J<0.6ASD, although the nucleation rate increases and the size of the grain 101 decreases as the current increases, the stress cannot meet the requirements, and the problem of lead 2 lifting and falling off after the bevel still exists.
[0071] Therefore, the circuit board manufacturing method provided in the embodiment of the present application is conducive to avoiding the problem of the lead 2 warping and falling off after the bevel, and preventing the fallen nickel-gold layer 14 from easily entering the welding surface, thereby reducing the risk of short circuit in the circuit board.
[0072] Please also read Fig. 9 and Fig.10 In some embodiments, the current density J is equal to 0.8ASD. At this current density, the electrochemical polarization effect is large, the cathode reaction overpotential is high, the critical radius of the crystal nucleus is reduced, the nucleation rate of the crystal increases, and the nucleation rate of the crystal is greater than the growth rate. Among them, when the current density J is equal to 0.8ASD, the nucleation rate is 1089 / (s·cm3) and reaches the highest, the grain size is 0.62um, and the porosity is 0.08 / (s·cm2) and is the smallest. At this time, the internal stress is in the best state.
[0073] Therefore, when the current density J is equal to 0.8ASD, the nucleation rate reaches the highest, the grain size is the smallest, and the porosity is the smallest. At this time, the internal stress is in the optimal state, which is more conducive to avoiding the problem of lead 2 warping and falling off after the bevel, thereby further reducing the risk of short circuit on the circuit board.
[0074] In some embodiments, when electroplating the gold finger 1 in the circuit board manufacturing method provided in the embodiment of the present application, the concentration of the brightener in the electroplating solution is n, and the value range of n is: 0.1%≤n≤0.3%.
[0075] See also Fig.11 , Fig.11 A in the middle is a schematic diagram of the inclined surface 11 of the gold finger 1 after electroplating with gold at a brightener concentration of 0.05%. Fig.11 b is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating with a brightener concentration of 0.1%. Fig.11 Figure c is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating with a brightener concentration of 0.2%. Fig.11 Figure d in the middle is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating with gold at a brightener concentration of 0.3%. Fig.11 Figure e is a schematic diagram of the bevel 11 of the gold finger 1 after electroplating with a brightener concentration of 0.35%. Fig.11 It can be seen that after the gold finger 1 was electroplated with gold at a brightener concentration of 0.05% in the electroplating solution, the nickel-gold point 141 did not fall off or warp, and the roughness Ra was 0.32um; after the gold finger 1 was electroplated with gold at a brightener concentration of 0.1% in the electroplating solution, the nickel-gold point 141 did not fall off or warp, and the roughness Ra was 0.25um; after the gold finger 1 was electroplated with gold at a brightener concentration of 0.2% in the electroplating solution, the nickel-gold point 141 did not fall off or warp, and the roughness Ra was 0.22um; after the gold finger 1 was electroplated with a brightener concentration of 0.3% in the electroplating solution, the nickel-gold point 141 did not fall off or warp, and the roughness Ra was 0.18um; after the gold finger 1 was electroplated with a brightener concentration of 0.34% in the electroplating solution, the nickel-gold point 141 warped, and the roughness Ra was 0.15um. Although the nickel-gold dots 141 did not fall off or lift up when the brightener concentration was 0.05%, the roughness Ra was too large, affecting the glossiness and smoothness of the finger.
[0076] In this way, the circuit board manufacturing method provided in the present application controls the brightener concentration within a reasonable range, ensures the softness of the electroplated layer while enhancing the gloss and smoothness, and can also ensure the uniformity and stability of the plating layer, which can reduce the brittleness of the nickel layer and help avoid the problem of lead 2 warping and falling off after the bevel, thereby reducing the risk of short circuit in the circuit board.
[0077] Exemplarily, the concentration of the brightener in the plating solution is n=0.2%.
[0078] In summary, the circuit board manufacturing method provided in the embodiment of the present application also controls the current density J within a reasonable range, and can obtain a gold-plated product with small pores and small grains, which can further reduce the internal stress of the nickel layer and thereby improve the nickel brittleness problem of the nickel-gold layer 14.
[0079] The inventors found that the internal stress in the coating is intrinsically linked to the electrocrystallization mechanism, grain size and porosity of the coating. Moderate grain size, low hydrogen permeation and low porosity all play a significant role in reducing internal stress. Therefore, changing nickel embrittlement can be optimized from the perspectives of grain size, porosity and hydrogen evolution.
[0080] Please also read Fig. 9 and Fig.12In some embodiments, in order to further reduce the internal stress of the nickel layer and thus improve the nickel brittleness problem of the nickel-gold layer 14, an embodiment of the present application provides a circuit board manufacturing method comprising the following steps:
[0081] S1, provide a substrate, the substrate has a gold finger 1 and a lead 2.
[0082] In step S1, the pre-process is completed according to the normal process to form a substrate, and then the subsequent processes are carried out. The pre-process includes: cutting, inner layer circuit, automated optical inspection (AOI), pressing, drilling target, milling edge, drilling, filling holes, circuit, solder mask, etc.
[0083] S2, electroplating gold on the gold finger 1. The current density of the electroplating gold is J, and the value range of J is: 0.6ASD≤J≤0.8ASD.
[0084] S3, baking the substrate, wherein the temperature of the baking plate is T, and the value range of T is: 150°C≤T≤180°C.
[0085] S4, beveling the gold finger 1 after the substrate is formed.
[0086] That is to say, on the basis of the previous embodiment, after electroplating the gold finger 1 and before beveling the gold finger 1 after the substrate is formed, the circuit board manufacturing method provided in the embodiment of the present application further includes:
[0087] The substrate is baked, wherein the temperature of the baking plate is T, and the value range of T is: 150°C≤T≤180°C.
[0088] In this way, the circuit board manufacturing method provided by the present application can release the hydrogen evolution effect during gold electroplating, evolve hydrogen from the pores of the lattice of the gold finger 1, reduce the internal stress of the nickel layer, and improve the nickel brittleness problem of the nickel-gold layer 14, thereby helping to avoid the problem of the lead 2 warping and falling off after the bevel, thereby reducing the risk of short circuit in the circuit board.
[0089] Please continue reading Fig.12 In some embodiments, in step S3 of the previous embodiment, the baking time is t, and the value range of t is: 60min≤t≤80min.
[0090] In this way, the circuit board manufacturing method provided by the present application can release the hydrogen evolution effect during gold electroplating, reduce the internal stress of the nickel layer, improve the nickel brittleness problem of the nickel-gold layer 14, and help avoid the problem of lead 2 warping and falling off after the bevel, thereby reducing the risk of short circuit in the circuit board.
[0091] For example, T=150° C., t=60 min. That is, when the circuit board manufacturing method provided in the present application bakes the substrate, the substrate is baked at a temperature of 150° C. for 60 min.
[0092] After the circuit board is baked, it is usually left to stand at room temperature, and then the board is cut into corresponding finished units by a gong machine, and then the bevel is performed. The inventor found that the conventional travel speed of the bevel is 4m / min, and the tool life is 10m. However, the current travel speed and tool life exert a certain external force on the nickel-gold layer 14, which easily causes the nickel-gold layer 14 to warp and fall off.
[0093] In some embodiments, when the circuit board manufacturing method provided by the present application is beveling the gold finger 1 after the substrate is formed, the moving speed of the gold finger 1 is v, and the value range of v is: 2m / min≤v≤3m / min.
[0094] The circuit board manufacturing method provided in the present application reduces the speed of the bevel, which can reduce the external force applied to the nickel-gold layer 14 during bevel, thereby helping to avoid the problem of the lead 2 warping or falling off after the bevel, thereby reducing the risk of short circuit in the circuit board.
[0095] Exemplarily, the moving speed of the golden finger 1 is v=2 m / min.
[0096] In some embodiments, when the circuit board manufacturing method provided by the present application performs beveling on the gold finger 1 after the substrate is formed, the life of the tool is L, and the value range of L is: 6m≤L≤8m.
[0097] In this way, the circuit board manufacturing method provided in the present application can reduce the life of the tool and reduce the external force applied to the nickel-gold layer 14 during beveling, thereby helping to avoid the problem of the lead 2 warping and falling off after beveling, thereby reducing the risk of short circuit in the circuit board.
[0098] For example, the tool life L=8m.
[0099] Please also read Fig.13 , Fig.14 and Fig.15 In some embodiments, the present application provides a circuit board manufacturing method comprising the following steps:
[0100] S1, provide a substrate, the substrate has a gold finger 1 and a lead 2.
[0101] In step S1, the pre-process is completed according to the normal process to form a substrate, and then the subsequent processes are carried out. The pre-process includes: cutting, inner layer circuit, automated optical inspection (AOI), pressing, drilling target, milling edge, drilling, filling holes, circuit, solder mask, etc.
[0102] S2, a gold-plating-resistant dry film 3 is provided on the substrate. When the gold-plating-resistant dry film 3 is provided on the substrate, a window is opened at the gold finger 1 and at a portion of the lead 2 close to the gold finger 1.
[0103] S3, electroplating gold on the gold finger 1. The current density of the electroplating gold is J, and the value range of J is: 0.6ASD≤J≤0.8ASD.
[0104] S4, baking the substrate. The temperature of the baking plate is T, and the value range of T is: 150°C≤T≤180°C. When stripping the film from the substrate, the dry film is stripped and cleaned by an organic stripping liquid.
[0105] S5, beveling the gold finger 1 after the substrate is formed.
[0106] That is to say, based on the previous embodiment, before the gold finger 1 is electroplated with gold, the circuit board manufacturing method provided by the present application also includes: setting an anti-gold plating dry film 3 on the substrate; wherein, when the anti-gold plating dry film 3 is set on the substrate, a window is opened at the gold finger 1 and at the part of the lead 2 close to the gold finger 1.
[0107] In this way, the circuit board manufacturing method provided in the present application allows the portion of the lead 2 close to the gold finger 1 to be electroplated with gold, thereby avoiding the situation where the lead 2 is not electroplated with gold due to deviation of the bevel equipment.
[0108] Please continue reading Fig.14 , for example, please refer to Fig.14 The lead 2 includes a non-windowed portion 21 and a windowed portion 22. The windowed portion 22 of the lead 2 includes a first side m and a second side n opposite to each other, the first side m is connected to the gold finger 1, the distance between the first side m and the second side n is d, and the value range of d is: 0.2mm≤d≤0.3mm.
[0109] In this way, the circuit board manufacturing method provided in the present application reserves a position for electroplating gold at the part of the lead 2 close to the gold finger 1, thereby avoiding the lead 2 not being electroplated gold due to deviation of the bevel equipment.
[0110] The embodiment of the present application also provides a circuit board, which is manufactured by the circuit board manufacturing method in the above embodiment. The circuit board provided by the present application has similar technical effects as the circuit board manufacturing method in the above embodiment, which will not be described in detail here.
[0111] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for manufacturing a circuit board, characterized in that: Providing a substrate, wherein the substrate has a gold finger; Electroplating the gold finger with gold, wherein the current density of the gold electroplating is J, and the value range of J is: 0.6ASD≤J≤0.8ASD; After the substrate is formed, the gold fingers are beveled.
2. The method for manufacturing a circuit board according to claim 1, wherein: The J is equal to 0.8 ASD.
3. The method for manufacturing a circuit board according to claim 1, wherein: After electroplating the gold fingers with gold and before beveling the gold fingers after forming the substrate, the method further includes: The substrate is baked, wherein the baking temperature is T, and the value range of T is: 150° C.≤T≤180° C.
4. The method for manufacturing a circuit board according to any one of claims 1 to 3, wherein: After electroplating the gold fingers with gold and before beveling the gold fingers after forming the substrate, the method further includes: The substrate is baked, wherein the baking time is t, and the value range of t is: 60min≤t≤80min.
5. The method for manufacturing a circuit board according to any one of claims 1 to 3, wherein: When electroplating the gold finger, the concentration of the brightener in the electroplating solution is n, and the value range of n is: 0.1%≤n≤0.3%.
6. The method for manufacturing a circuit board according to claim 1, wherein: When the gold finger is beveled after the substrate is formed, the moving speed of the gold finger is set to v, and the value range of v is: 2m / min≤v≤3m / min.
7. The method for manufacturing a circuit board according to claim 1, 2, 3 or 6, wherein: When the gold finger is beveled after the substrate is formed, the life of the tool is set to L, and the value range of L is: 6m≤L≤8m.
8. The method for manufacturing a circuit board according to claim 1, wherein: The substrate further has a lead connected to one end of the gold finger. Before electroplating gold on the gold finger, the method further comprises: providing a gold-plating-resistant dry film on the substrate. When the gold-plating-resistant dry film is provided on the substrate, a window is opened at the gold finger and at a portion of the lead close to the gold finger.
9. The method for manufacturing a circuit board according to claim 8, wherein: The window portion of the lead includes a first side and a second side opposite to each other, the first side is connected to the gold finger, the distance between the first side and the second side is d, and the value range of d is: 0.2mm≤d≤0.3mm.
10. A circuit board, characterized in that: The circuit board is manufactured by the circuit board manufacturing method according to any one of claims 1 to 9.
Citation Information
Cited By
Conductive structure preparation method, conductive structure and micro electro mechanical system
CN119822321A