Self-supporting ferroelectric film with wrinkle structure and preparation method thereof
By growing a soluble sacrificial layer between the ferroelectric layer and the substrate, the ferroelectric layer is peeled off from the original substrate and transferred to the silicon nano-island array to form a wrinkled self-supporting ferroelectric thin film. This solves the problem of combining ferroelectric thin films with semiconductor processes in the prior art and achieves high-quality ferroelectricity and application expansion.
Patent Information
- Application Number
- CN202410953529.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for preparing ferroelectric thin films are difficult to integrate effectively with semiconductor processes, and traditional methods are costly and polluting, limiting their application in nanoelectronic devices.
By growing a soluble sacrificial layer between the ferroelectric layer and the substrate, the ferroelectric layer is peeled off from the original substrate and transferred to the silicon nanoisland array using its solubility, forming a self-supporting ferroelectric thin film with a wrinkled structure, thus achieving integration with silicon-based semiconductor processes.
The prepared self-supporting ferroelectric thin film has high crystallinity and excellent ferroelectricity, which breaks through the substrate limitation and realizes the combination with silicon-based semiconductor technology, providing more possibilities for the application of ferroelectric thin films in nanoelectronic devices.
Smart Images

Figure CN118922056A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano ferroelectric materials, and in particular to a self-supporting ferroelectric film with a folded structure and a preparation method thereof. Background Art
[0002] At present, metal oxide thin film materials are widely studied, developed and used due to many novel light, electricity, force, heat and other response effects found in them. Among them, ferroelectric thin film materials have aroused the research interests of scientific research enthusiasts due to their excellent piezoelectricity, pyroelectricity, ferroelectricity, dielectricity and photoelectric effects, and have shown great application prospects in the field of nanoelectronic devices.
[0003] Since the development of ferroelectric thin film materials in 1977, various high-quality preparation methods have been formed. Among them, sol-gel method, magnetron sputtering method, pulsed laser deposition method and chemical vapor deposition method are the more mainstream preparation processes at present. There is no doubt that the progress of thin film preparation technology has an indispensable role in promoting the development of ferroelectric materials. Therefore, it is of great significance to continuously optimize the preparation process of ferroelectric thin films for their application in nanoelectronic devices.
[0004] At present, the preparation process of high-quality ferroelectric thin films is relatively mature, but its effective combination with traditional semiconductor materials and processes is a hot issue at present. Many scientific researchers are committed to improving the preparation method of ferroelectric thin film materials to meet the requirements of miniaturization and integration in current semiconductor processes. For example, pulsed laser deposition technology is used to grow ferroelectric thin films. This method can grow high-quality epitaxial single crystal films, but it usually requires a substrate as a support, which greatly limits its integration with modern semiconductor processes; another example is the use of chemical vapor deposition technology to prepare high-quality ferroelectric thin films, but the raw materials and equipment required for this method are relatively expensive, and the preparation process is accompanied by toxicity and pollution, which limits the scope of application. Therefore, a method for preparing ferroelectric thin films that meets current semiconductor processes has practical significance for the wide application of ferroelectric thin films in nanoelectronic devices. Summary of the invention
[0005] Based on this, the purpose of the present invention is to provide a self-supporting ferroelectric film with a corrugated structure and a preparation method thereof, which uses a substrate transfer technology to peel off the ferroelectric film from the substrate and transfer it to a silicon-based semiconductor to form a self-supporting ferroelectric film with a corrugated structure. This process provides a new idea for further promoting the application of ferroelectric films.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a self-supporting ferroelectric film having a corrugated structure, comprising the following steps:
[0008] A Sr2CaAl2O6 film was deposited as a sacrificial layer on a (001) oriented SrTiO3 single crystal substrate;
[0009] Depositing a SrRuO3 conductive layer on the sacrificial layer as a bottom electrode;
[0010] depositing a rhombohedral ferroelectric thin film on the bottom electrode;
[0011] After dissolving the sacrificial layer, the film sample is transferred to the silicon nano-island array to obtain a self-supporting ferroelectric film with a wrinkled structure.
[0012] Compared with the prior art, the present invention grows a sacrificial layer between the ferroelectric layer and the substrate, utilizes the property of the sacrificial layer being soluble in water, peels the ferroelectric layer off the original substrate, and then re-transfers it to the silicon nano-island array. Due to the supporting effect of the silicon nano-island array, a regular and orderly large-area wrinkle structure is formed. The wrinkle structure introduces a strain gradient, and the strain gradient generates flexoelectricity, which is conducive to domain control on the ferroelectric film through the flexoelectric effect. After testing, the self-supporting ferroelectric film with a wrinkle structure prepared by the present invention has high crystallinity and excellent ferroelectricity. The preparation method of the self-supporting ferroelectric film with a wrinkle structure proposed by the present invention can enable the ferroelectric film to break through the barrier of substrate limitation, realize the combination with silicon-based semiconductor technology, and provide more possibilities for the application of ferroelectric film materials. This method is applicable to a variety of ferroelectric materials, even multifunctional oxide films, and has great practical significance.
[0013] In a preferred embodiment, the thickness of the sacrificial layer is 20-50 nm, which not only has a sufficient film thickness, but also facilitates the subsequent dissolution step.
[0014] In a preferred embodiment, the sacrificial layer is deposited by pulse laser deposition technology, and the experimental conditions are: pulse energy of 62-66 mJ, pulse frequency of 1-8 Hz, epitaxial temperature of 750-780° C., and oxygen pressure of 4-10 Pa. Under the above experimental conditions, a sacrificial layer with uniform thickness, smooth surface and easy dissolution can be deposited.
[0015] In a preferred embodiment, the sacrificial layer is dissolved by immersion in deionized water. By utilizing the water-soluble property of the sacrificial layer material (Sr2CaAl2O6), the sacrificial layer can be easily dissolved by immersing the sample in deionized water, thereby peeling the ferroelectric layer from the original substrate.
[0016] In a preferred embodiment, the sacrificial layer is dissolved after being soaked in deionized water for 10 to 24 hours, and then the floating film is picked up by the silicon nano-island array to obtain a self-supporting ferroelectric film with a folded structure. Since the thickness of the sacrificial layer is controlled within a suitable size range, the dissolution time is short and it can be completely dissolved after 10 to 24 hours. After dissolution, the film floating on the surface of the deionized water is picked up by the silicon nano-island array. Since the film is closely attached to the silicon nano-island array on the surface of the silicon wafer, a self-supporting ferroelectric film with a folded structure can be obtained.
[0017] In a preferred embodiment, the thickness of the bottom electrode is 6-10 nm; the bottom electrode is deposited by pulse laser deposition technology, and the experimental conditions are: pulse energy is 75-90 mJ, pulse frequency is 8 Hz, epitaxial temperature is 660-720° C., and oxygen pressure is 15-20 Pa. Under the experimental conditions, a uniform and flat bottom electrode can be obtained.
[0018] In a preferred embodiment, the ferroelectric thin film is a BFO (BiFeO3) thin film. In other embodiments, the ferroelectric thin film may also be made of other metal oxide thin film materials.
[0019] In a preferred embodiment, the thickness of the BFO film is 10-25 nm; the BFO film is epitaxially grown on the bottom electrode by pulsed laser deposition technology, and the experimental conditions are: pulse energy is 62-66 mJ, pulse frequency is 8 Hz, epitaxial temperature is 710-730°C, and oxygen pressure is 15-20 Pa. The BFO film grown by this method and experimental conditions has good epitaxy, a clean and flat surface, uniform thickness, and good ferroelectricity.
[0020] In a preferred embodiment, the silicon nano-island array is prepared by the following steps: a 500nm single-layer densely packed polystyrene sphere template is spread on a silicon wafer by an aqueous solution method, and a mask is formed after drying; the sample is then treated with oxygen plasma in an oxygen atmosphere and a power of 65 to 80W, so that the diameter of the PS sphere changes from the initial 500nm to about 300nm, thereby obtaining PS sphere templates separated from each other; the sample is then argon ion beam etched to etch away the portion not blocked by the PS sphere; and finally, the PS sphere template is removed by ultrasonic cleaning to obtain an orderly arranged silicon nano-island array.
[0021] In a second aspect, the present invention further provides a self-supporting ferroelectric film with a corrugated structure prepared by a method as described in any one of the above embodiments, which has high crystallinity and excellent ferroelectric properties.
[0022] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1A flow chart of a method for preparing a self-supporting ferroelectric thin film with a corrugated structure in one embodiment of the present invention;
[0024] Figure 2 This is the morphology of the BFO film before peeling in Example 1;
[0025] Figure 3 This is the morphology of the BFO film after peeling off in Example 1;
[0026] Figure 4 The piezoelectric loop diagram of the self-supporting ferroelectric film obtained in Example 1;
[0027] Figure 5 The SEM image (2500 times) of the self-supporting ferroelectric thin film prepared in Example 1;
[0028] Figure 6 This is the SEM image (10,000 times) of the free-standing ferroelectric thin film prepared in Example 1. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0030] The self-supporting ferroelectric film with a corrugated structure provided by the present invention and its preparation method and application are described in detail below.
[0031] The present invention provides a method for preparing a self-supporting ferroelectric film with a corrugated structure, comprising the following steps:
[0032] A Sr2CaAl2O6 film was deposited as a sacrificial layer on a (001) oriented SrTiO3 single crystal substrate;
[0033] Depositing a SrRuO3 conductive layer on the sacrificial layer as a bottom electrode;
[0034] depositing a rhombohedral ferroelectric thin film on the bottom electrode;
[0035] After dissolving the sacrificial layer, the film sample is transferred to the silicon nano-island array to obtain a self-supporting ferroelectric film with a wrinkled structure.
[0036] Further, the thickness of the sacrificial layer is 20-50 nm. Exemplarily, the thickness of the sacrificial layer can be 20 nm, 30 nm, 40 nm or 50 nm, or any other value within the range of 20-50 nm.
[0037] For reference, the sacrificial layer is deposited by pulsed laser deposition technology. Pulsed laser deposition is a method of using high-energy laser pulses generated by a laser to evaporate the target material and deposit a film on the substrate. The experimental conditions are: pulse energy of 62-66mJ, pulse frequency of 1-8Hz, epitaxial temperature of 750-780°C, and oxygen pressure of 4-10Pa. Exemplarily, the pulse energy can be 62mJ, 63mJ, 64mJ, 65mJ or 66mJ, or any other value in the range of 62-66mJ. The pulse frequency can be 1Hz, 2Hz, 3Hz, 4Hz, 5Hz, 6Hz, 7Hz or 8Hz, or any other value in the range of 1-8Hz. The epitaxial temperature can be 750°C, 7600°C, 770°C or 780°C, or any other value in the range of 750-780°C. The oxygen pressure may be 4Pa, 5Pa, 6Pa, 7Pa, 8Pa, 9Pa or 10Pa, or any other value within the range of 4 to 10Pa.
[0038] For reference, the sacrificial layer is dissolved by soaking in deionized water. The sacrificial layer is dissolved after soaking in deionized water for 10 to 24 hours, and then the floating film is picked up with a silicon nano-island array to obtain a self-supporting ferroelectric film with a pleated structure. Exemplarily, the soaking time can be 10 hours, 12 hours, 15 hours, 18 hours, 20 hours or 24 hours, or any other value within the range of 10 to 24 hours, as long as the sacrificial layer is completely dissolved in deionized water. After dissolution, the film floating on the surface of deionized water can be picked up with a silicon nano-island array. Since the film fits tightly with the silicon nano-island array on the surface of the silicon wafer, a self-supporting ferroelectric film with a pleated structure can be obtained.
[0039] For reference, the thickness of the bottom electrode is 6 to 10 nm. Exemplarily, the thickness of the bottom electrode can be 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc., or any other value within the range of 6 to 20 nm. The bottom electrode is deposited by pulsed laser deposition technology, and the experimental conditions are: pulse energy of 70 to 90 mJ, pulse frequency of 8 Hz, epitaxial temperature of 660 to 720 ° C, and oxygen pressure of 15 to 20 Pa. Exemplarily, the pulse energy can be 70 mJ, 80 mJ or 90 mJ, or any other value within the range of 70 to 90 mJ. The epitaxial temperature can be 660 ° C, 680 ° C, 700 ° C or 720 ° C, or any other value within the range of 660 to 720 ° C. The oxygen pressure can be 15 Pa, 16 Pa, 17 Pa, 18 Pa, 19 Pa or 20 Pa, or any other value within the range of 15 to 20 Pa.
[0040] For reference, the ferroelectric film is a BFO (BiFeO3) film. In other embodiments, the ferroelectric film may also be made of other metal oxide film materials, such as PTO (PbTiO3) film, STO (SrTiO3) film, BTO (BaTiO3) film, SRO (SrRuO3) film, etc.
[0041] For reference, the thickness of the BFO film is 10 to 25 nm. For example, the thickness of the BFO film can be 10 nm, 15 nm, 20 nm or 25 nm, or any other value within the range of 10 to 25 nm. The BFO film is epitaxially grown on the bottom electrode by pulsed laser deposition technology. The experimental conditions are: pulse energy of 62 to 66 mJ, pulse frequency of 8 Hz, epitaxial temperature of 710 to 730 ° C, and oxygen pressure of 15 to 20 Pa. For example, the pulse energy can be 62 mJ, 63 mJ, 64 mJ, 65 mJ or 66 mJ, or any other value within the range of 62 to 66 mJ. The epitaxial temperature can be 710 ° C, 720 ° C or 730 ° C, or any other value within the range of 710 to 730 ° C. The oxygen pressure can be 15 Pa, 16 Pa, 17 Pa, 18 Pa, 19 Pa or 20 Pa, or any other value within the range of 15 to 20 Pa.
[0042] For reference, the silicon nano-island array is made by the following steps: a monolayer of 500nm densely packed polystyrene sphere template is spread on a silicon wafer by an aqueous solution method, and a mask is formed after drying; then the sample is treated with oxygen plasma in an oxygen atmosphere and a power of 65 to 80W, so that the diameter of the PS sphere changes from the initial 500nm to about 300nm, and a PS sphere template separated from each other is obtained; then the sample is etched by an argon ion beam to etch away the part not blocked by the PS sphere; finally, after ultrasonic cleaning to remove the PS sphere template, an orderly arranged silicon nano-island array is obtained. Exemplarily, the power of the oxygen plasma treatment can be 65W, 70W, 75W or 80W, or any other value within the range of 65 to 80W.
[0043] Accordingly, the present invention also provides a self-supporting ferroelectric film with a corrugated structure prepared by a method as in any of the above embodiments, wherein the corrugated structure introduces a strain gradient, and the strain gradient generates flexoelectricity, which is conducive to domain control on BFO through the flexoelectric effect. After testing, the self-supporting ferroelectric film with a corrugated structure provided by the present invention has high crystallinity and excellent ferroelectricity.
[0044] The following is the best embodiment of the present invention. It should be noted that the various parameter values used in the embodiments are all preferred parameter values within the parameter range limited by the claims. In other embodiments, as long as the adopted parameter values are within the scope of the claims, the purpose of the present invention can be achieved.
[0045] Example 1
[0046] This embodiment provides a self-supporting ferroelectric film with a corrugated structure and a preparation method thereof, such as Figure 1 As shown, the following steps are included:
[0047] S1: Preparation of silicon nano-island array: A single layer of 500nm densely packed polystyrene (PS) ball template is spread on a silicon wafer using an aqueous solution method. After drying, the ball is firmly in contact with the surface of the silicon wafer to form a mask. Then the sample is treated with PLASMA in an oxygen atmosphere and 60W power for 60 minutes, so that the diameter of the PS ball changes from the initial 500nm to about 300nm, thereby obtaining PS ball templates separated from each other. The sample is further etched by argon ion beam, and the anode current is 1.1A for 120S. The part not blocked by the PS ball is etched away, while the part covered by the PS ball is retained. The etching time here is determined by the etching resistance of the material itself and the required etching depth. Finally, in an ultrasonic cleaner, chloroform, anhydrous ethanol, deionized water and other solutions are used to clean for 15min, 10min, and 5min at a frequency of 90Hz, respectively. After removing the PS ball template, an orderly arranged silicon nano-island array is obtained.
[0048] S2: Select a (001) oriented STO (SrTiO3) target, and use pulsed laser deposition to deposit a SCAO (Sr2CaAl2O6) film as a sacrificial layer on the STO target. Specifically, a 30nm thick SCAO (Sr2CaAl2O6) film is grown as a sacrificial layer under the experimental conditions of pulse energy of 63mJ, pulse frequency of 5Hz, epitaxial temperature of 780℃, and oxygen pressure of 4Pa.
[0049] S3: Preparation of bottom electrode: Under the experimental conditions of pulse energy of 78 mJ, pulse frequency of 8 Hz, temperature of 680°C and oxygen pressure of 15 Pa, a 8 nm thick SRO (SrRuO3) conductive layer is grown on the sacrificial layer as the bottom electrode.
[0050] S4: Select a BFO (BiFeO3) target material, and use a pulsed laser deposition method to deposit a rhombohedral BFO film on the SRO bottom electrode prepared in step S3. Specifically, a 20nm thick BiFeO3 (BFO) film is epitaxially grown under the experimental conditions of a pulse energy of 66mJ, a pulse frequency of 8Hz, a temperature of 730°C, and an oxygen pressure of 15Pa.
[0051] S5: placing the sample obtained in S4 in a beaker filled with deionized water and soaking it for 10 to 24 hours until the sacrificial layer is completely dissolved, and then using the silicon nano-island array obtained in step S1 to pick up the floating film, a self-supporting ferroelectric film with a wrinkled structure can be obtained.
[0052] S6: Use piezoelectric force microscopy to test the morphology and domain structure of the samples.
[0053] Piezoelectric force microscopy is a microscope developed on the basis of contact mode atomic force microscopy that detects the amount of electro-induced deformation on the sample surface at a microscopic scale. This mode is mainly used to characterize the domain structure of ferroelectric materials and detect the mechanical deformation of the sample caused by the inverse piezoelectric effect under an applied electric field. By applying an AC voltage to the conductive needle tip, the local sample under the needle tip undergoes periodic deformation. This deformation causes the cantilever connected to the needle tip to twist, thereby affecting the optical signal reflected by it. This signal is collected by the photodiode and subsequently analyzed by the lock-in amplifier to achieve detection. At the same time, the needle tip can also apply a DC bias during contact scanning with the sample to flip the polarization of the ferroelectric material. Here, the piezoresistance force microscope is used to characterize the morphology of the peeled BFO film. The results show that the surface of the BFO film is well bonded to the silicon wafer surface, and the film surface forms a large area of wrinkled structure due to the highly ordered nano-island array on the silicon wafer.
[0054] Figure 2 and 3 They are AFM morphology images of the BFO film in Example 1 before and after peeling. It can be seen from the figures that the surface of the BFO film is smooth and wrinkle-free before peeling, and the surface of the BFO film after peeling forms a regular and orderly wrinkle structure due to the support of Si nano-islands, with an average height of about 25 nm.
[0055] Figure 4 This is the piezoelectric loop diagram of the self-supporting BFO film prepared in Example 1. The test results show that the self-supporting BFO film has high crystallinity and excellent ferroelectricity.
[0056] Figure 5 and Figure 6The SEM microscope images of the self-supporting BFO film prepared in Example 1 are at magnifications of 2500 and 10000 respectively. It can be seen from the images that a large area of wrinkled structure is formed on the surface of the self-supporting BFO film, and the wrinkled structure is highly ordered.
[0057] In summary, compared with the prior art, the present invention grows a sacrificial layer between the ferroelectric layer and the substrate, utilizes the property that the sacrificial layer can be dissolved in water, peels the ferroelectric layer off the original substrate, and then re-transfers it to the silicon nano-island array. Due to the supporting effect of the silicon nano-island array, a regular and orderly large-area wrinkle structure is formed. The wrinkle structure introduces a strain gradient, and the strain gradient produces flexoelectricity, which is conducive to domain regulation on the ferroelectric film through the flexoelectric effect. After testing, the self-supporting ferroelectric film with a wrinkle structure prepared by the present invention has high crystallinity and excellent ferroelectricity. The preparation method of the self-supporting ferroelectric film with a wrinkle structure proposed by the present invention can enable the ferroelectric film to break through the barrier of substrate limitation, realize the combination with silicon-based semiconductor technology, and provide more possibilities for the application of ferroelectric film materials. This method is applicable to a variety of ferroelectric materials, even multifunctional oxide films, and has great practical significance.
[0058] The above-mentioned embodiment only expresses one implementation mode of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a self-supporting ferroelectric thin film with a corrugated structure, characterized in that: The following steps are involved: preparing silicon nano-island arrays; A Sr2CaAl2O6 film was deposited as a sacrificial layer on a (001) oriented SrTiO3 single crystal substrate; Depositing a SrRuO3 conductive layer on the sacrificial layer as a bottom electrode; Depositing a rhombohedral ferroelectric thin film on the bottom electrode; After dissolving the sacrificial layer, the film sample is transferred to the silicon nano-island array to obtain a self-supporting ferroelectric film with a wrinkled structure.
2. The preparation method according to claim 1, characterized in that: The thickness of the sacrificial layer is 20-50 nm.
3. The preparation method according to claim 2, characterized in that: The sacrificial layer is deposited by pulse laser deposition technology, and the experimental conditions are: pulse energy is 62-66 mJ, pulse frequency is 1-8 Hz, epitaxial temperature is 750-780° C., and oxygen pressure is 4-10 Pa.
4. The preparation method according to claim 1, characterized in that: The sacrificial layer is dissolved by soaking in deionized water.
5. The preparation method according to claim 4, characterized in that: The sacrificial layer is dissolved after being immersed in deionized water for 10 to 24 hours, and then the floating film is picked up by a silicon nano-island array to obtain a self-supporting ferroelectric film with a folded structure.
6. The preparation method according to claim 1, characterized in that: The thickness of the bottom electrode is 6-10 nm; the bottom electrode is deposited by pulse laser deposition technology, and the experimental conditions are: pulse energy is 75-90 mJ, pulse frequency is 8 Hz, epitaxial temperature is 660-720° C., and oxygen pressure is 15-20 Pa.
7. The preparation method according to claim 1, characterized in that: The ferroelectric film is a BFO film.
8. The preparation method according to claim 7, characterized in that: The thickness of the BFO film is 10-25 nm; the BFO film is epitaxially grown on the bottom electrode by pulse laser deposition technology, and the experimental conditions are: pulse energy is 62-66 mJ, pulse frequency is 8 Hz, epitaxial temperature is 710-730° C., and oxygen pressure is 15-20 Pa.
9. The preparation method according to claim 1, characterized in that: The silicon nano-island array is prepared by the following steps: a single layer of 500nm densely packed polystyrene sphere template is spread on a silicon wafer by an aqueous solution method, and a mask is formed after drying; the sample is then treated with oxygen plasma in an oxygen atmosphere and a power of 65 to 80W, so that the diameter of the PS sphere changes from the initial 500nm to about 300nm, thereby obtaining PS sphere templates separated from each other; the sample is then etched by argon ion beam to etch away the part not blocked by the PS sphere; and finally, the PS sphere template is removed by ultrasonic cleaning to obtain an orderly arranged silicon nano-island array.
10. A self-supporting ferroelectric film with a corrugated structure, characterized in that: The preparation method is as described in any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of ferroelectric memory
CN119866015A
Multi-layer thin film capacitor based on strain effect
CN120637106A
A multilayer thin film capacitor based on strain effect
CN120637106B
Self-supporting device with multilayer metal electrode structure and preparation method thereof
CN121692832A
Flexible piezoelectric sensing drive device and preparation method thereof
CN122421659A