Inkjet recording method

By imparting ink on the A surface of the paper substrate and irradiating infrared rays, combined with post-treatment liquid that imparts surfactant on the B surface, the problem of cracks when bending the image recorder is solved, and better fold resistance is achieved and rub resistance.

CN118922314APending Publication Date: 2024-11-08FUJIFILM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380029852.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-01-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When bending the image recording object, the prior art is difficult to effectively suppress the occurrence of cracks, especially when recording with aqueous ink, uneven drying of the ink causes the paper substrate to become brittle and cracks are prone to occur.

Method used

By using the inkjet recording method, an ink containing a colorant and water is applied to the A surface of the paper substrate, and infrared irradiation is applied to the range of 800 nm to 3,000 nm; after which a water and surfactant is applied to the B surface, the ink containing a water and a surfactant is applied to the A surface of the paper. The treatment liquid, the coating includes calcium carbonate and kaolin, and the coating on the B-side side has a small amount of dry coating for the post-treatment liquid to penetrate.

Benefits of technology

The cracks generated when bending the image recording object are effectively suppressed, and the image resistance to folding and rubbing resistance is improved, while maintaining the strength of the image recording object.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056685270000261
    Figure BDA0005056685270000261
  • Figure BDA0005056685270000291
    Figure BDA0005056685270000291
  • Figure BDA0005056685270000311
    Figure BDA0005056685270000311
Patent Text Reader

Abstract

An ink jet recording method includes, in order: a step of applying an ink containing a colorant and water to a surface A, which is one surface of a paper substrate, by means of an ink jet recording method; a step for irradiating the surface A to which the ink is applied with infrared rays having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step for applying a post-treatment liquid containing water and a surfactant to a surface B, which is the other surface of the paper substrate, the paper substrate comprising a pulp layer and a coating layer, the coating layer being disposed on the surface A side, the dry coating amount of the coating layer disposed on the surface A side being 15-50 g / m2, and the surface B being a surface B of the paper substrate when the coating layer is not disposed on the surface B side or when the coating layer is disposed on the surface B side, the dry coating amount of the coating layer disposed on the surface A side being 15-50 g / m2. The dry coating amount of the coating layer disposed on the B-surface side is 10 g / m2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an inkjet recording method. Background Art

[0002] In recent years, in the method of recording an image using aqueous ink containing water, research has been conducted on improving various properties of the image recorded material obtained.

[0003] For example, Japanese Patent Publication No. 2017-124561 describes an image forming method that forms an image by ejecting droplets onto a recording medium, characterized in that a post-processing liquid is ejected onto an image of at least a recording medium on which an image is formed, an area overlapping with an area of ​​the recording medium on which an image is formed is determined, and the post-processing liquid is ejected onto the determined area. Japanese Patent Publication No. 2020-164333 describes a post-processing device, characterized in that it comprises: a post-processing unit that performs post-processing of a recording medium recorded using aqueous ink; a loading unit that loads the recording medium that has been post-processed by the post-processing unit; a deformation suppression mechanism that suppresses deformation of the recording medium in the loading unit caused by a specified parameter involved in the recording process of the recording medium; and a control unit that controls the deformation suppression mechanism according to the specified parameter, the control unit receives the specified parameter from a printer control unit that controls the recording, and changes the suppression strength of the deformation suppression mechanism on the recording medium according to the specified parameter, wherein the specified parameter includes information based on the conditions when recording is performed on the recording medium. Summary of the invention

[0004] Technical issues to be solved by the invention

[0005] However, there is a case where it is required to suppress the generation of cracks when the image recorded material is bent.

[0006] The present invention has been made in view of such circumstances, and according to one embodiment of the present invention, an inkjet recording method capable of suppressing the generation of cracks when an image recorded material is bent is provided.

[0007] Means for solving technical problems

[0008] The present invention includes the following aspects.

[0009] <1>

[0010] An inkjet recording method, comprising:

[0011] A step of applying ink containing a colorant and water to one side of a paper substrate, namely side A, by an inkjet recording method;

[0012] A step of irradiating the surface A provided with ink with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; and

[0013] A step of applying a post-treatment liquid containing water and a surfactant to the other side of the paper substrate, namely, side B,

[0014] The paper substrate comprises a pulp layer and a coating layer disposed on at least one surface of the pulp layer.

[0015] The coating comprises at least one white pigment selected from the group consisting of calcium carbonate and kaolin and a binder,

[0016] A coating layer is arranged on the A surface side, and the dry coating amount of the coating layer arranged on the A surface side is 15 g / m 2 ~50g / m 2 ,

[0017] When the coating layer is not disposed on the B side or is disposed on the B side, the dry coating amount of the coating layer disposed on the B side is 10 g / m 2 the following.

[0018] <2> The inkjet recording method according to <1>, wherein

[0019] Infrared rays are near-infrared rays having a maximum wavelength in the range of 800 nm to 1,400 nm.

[0020] <3>

[0021] The inkjet recording method according to <1> or <2>, wherein:

[0022] The surface tension of the post-treatment liquid is 22.5 mN / m to 40.0 mN / m.

[0023] <4>

[0024] The inkjet recording method according to any one of <1> to <3>, wherein

[0025] In the step of applying the post-treatment liquid, the amount applied per unit area is 10 g / m 2 ~55g / m 2 The range is given to the post-treatment liquid.

[0026] <5>

[0027] The inkjet recording method according to any one of <1> to <4>, wherein

[0028] The surfactant includes a nonionic surfactant.

[0029] <6>

[0030] The inkjet recording method according to any one of <1> to <5>, wherein

[0031] The HLB value of the surfactant is 8.0 to 14.0.

[0032] <7>

[0033] The inkjet recording method according to any one of <1> to <6>, wherein

[0034] The basis weight of the paper substrate is 180g / m 2 ~600g / m 2 .

[0035] <8>

[0036] The inkjet recording method according to any one of <1> to <7>, comprising:

[0037] Before applying the ink, a pre-treatment liquid is applied to the A surface.

[0038] In the ink application step, ink is applied to the surface A to which the pretreatment liquid has been applied.

[0039] <9>

[0040] The inkjet recording method according to <8>, wherein

[0041] The pretreatment solution contains an organic acid.

[0042] Effects of the Invention

[0043] According to one embodiment of the present invention, there is provided an inkjet recording method capable of suppressing the generation of cracks when an image recorded material is folded. DETAILED DESCRIPTION

[0044] Hereinafter, the inkjet recording method of the present invention will be described in detail.

[0045] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0046] In the numerical ranges recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical ranges recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiments.

[0047] In the present specification, when a plurality of substances corresponding to each component are present in a composition, the amount of each component in the composition refers to the total amount of the plurality of substances present in the composition unless otherwise specified.

[0048] In the present specification, a combination of two or more preferred aspects is a more preferred aspect.

[0049] In the present specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0050] In this specification, "image" refers to the entire film, and "image recording" refers to the formation of an image (ie, film). Furthermore, the concept of "image" in this specification also includes a solid image.

[0051] In this specification, “(meth)acrylate” is a concept including both acrylate and methacrylate, “(meth)acryloyl” is a concept including both acryloyl and methacryloyl, and “(meth)acrylic acid” is a concept including both acrylic acid and methacrylic acid.

[0052] [Inkjet recording method]

[0053] The inkjet recording method of the present invention comprises: a step of applying ink containing a colorant and water to one side, i.e., side A, of a paper substrate by inkjet recording; a step of irradiating the side A to which the ink has been applied with infrared rays having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step of applying a post-treatment liquid containing water and a surfactant to the other side, i.e., side B, of the paper substrate, wherein the paper substrate comprises a pulp layer and a coating layer disposed on at least one side of the pulp layer, the coating layer comprising at least one white pigment selected from the group consisting of calcium carbonate and kaolin and a binder, the coating layer being disposed on the side A, and the dry coating amount of the coating layer disposed on the side A being 15 g / m 2 ~50g / m 2 In the case where the coating is not disposed on the B side or is disposed on the B side, the dry coating amount of the coating disposed on the B side is 10 g / m 2 the following.

[0054] As a result of intensive research, the present inventors have found that the inkjet recording method according to the present invention can suppress the generation of cracks when an image recorded material is folded. The reason for achieving such an effect is presumably as follows.

[0055] Infrared rays have a large energy density and high drying efficiency. However, if after ink is applied to a paper substrate, the surface (surface A) applied with ink is irradiated with infrared rays, the water contained in the paper substrate will also volatilize, and the image recorded material itself will become brittle, and there is a tendency for cracks to easily occur in the coating layer and the underlying pulp layer when the image recorded material is bent. In particular, water is easy to volatilize in the area on the paper substrate that is not applied with ink. In addition, when multiple inks with different hues are applied, the degree of drying of each ink will be different due to the differences in the absorption spectra of the inks. For example, compared with inks of hues such as yellow, magenta, and cyan, black ink absorbs more infrared rays, so water is easy to volatilize in the area applied with black ink. In the area where no ink is applied and the area where black ink is applied, there is a tendency for cracks to occur more easily when the image recorded material is bent.

[0056] In contrast, in the inkjet recording method of the present invention, a post-treatment liquid containing water and a surfactant is applied to the surface (surface B) of the paper substrate opposite to the surface (surface A) to which the ink is applied. By allowing the post-treatment liquid to penetrate the surface B of the paper substrate, the generation of cracks can be suppressed when the image recorded material is bent.

[0057] In the image forming method described in Japanese Patent Publication No. 2017-124561, a post-processing liquid is ejected onto an image on a recording medium on which an image is formed. Japanese Patent Publication No. 2020-164333 does not contain any description of a post-processing liquid containing water and a surfactant. Japanese Patent Publication No. 2017-124561 and Japanese Patent Publication No. 2020-164333 do not envision bending the image recorded material.

[0058] Hereinafter, the paper substrate and each step used in the inkjet recording method according to the present invention will be described in detail.

[0059] <Paper base material>

[0060] The inkjet recording method of the present invention includes: a step of applying an ink containing a pigment and water to one side of a paper substrate, namely side A, by an inkjet recording method; and a step of applying a post-treatment liquid containing water and a surfactant to the other side of the paper substrate, namely side B. That is, side A of the paper substrate is the side to which the ink is applied. Side B of the paper substrate is the side to which the post-treatment liquid is applied.

[0061] The paper substrate used in the inkjet recording method according to the present invention includes a pulp layer and a coating layer disposed on at least one surface of the pulp layer.

[0062] The pulp layer may be only one layer or two or more layers may be stacked.

[0063] The pulp layer is a layer containing pulp as a main component. Here, the main component refers to a component that accounts for 50% by mass or more of the components constituting the pulp layer.

[0064] The type of pulp is not particularly limited, but from the viewpoint of strength, the pulp layer preferably contains chemical pulp. Examples of chemical pulp include broadleaf kraft pulp (LKP) and coniferous kraft pulp (NKP).

[0065] The pulp may be sun-dried pulp or unsun-dried pulp. LKP and NKP may be sun-dried pulp or unsun-dried pulp, respectively.

[0066] As other pulps besides the above-mentioned NKP and LKP, for example, there can be mentioned: mechanical pulps such as stone ground pulp (SGP), pressure stone ground pulp (PGW), wood chip ground pulp (RGP), thermal ground pulp (TGP), chemical ground pulp (CGP), ground pulp (GP), thermomechanical pulp (TMP); decomposed waste paper pulp (DIP) produced from waste tea paper, waste kraft envelope paper, waste magazines, waste newspapers, waste flyers, waste office paper, waste corrugated paper, waste white paper, waste Kent paper, waste imitation paper, waste land certificate, etc.; and pulp chemically or mechanically produced from non-wood fibers such as kenaf, hemp, and reed.

[0067] The coating layer may be disposed on both surfaces of the pulp layer, or may be disposed on only one surface of the pulp layer.

[0068] In the paper substrate, a coating layer is arranged on the A side, and the dry coating amount of the coating layer arranged on the A side is 15 g / m 2 ~50g / m 2 When the coating is not arranged on the B side or is arranged on the B side, the dry coating amount of the coating arranged on the B side is 10 g / m 2 Therefore, when the coating is arranged on both sides of the pulp layer, the side where the coating with a larger dry coating amount is arranged is the A side (i.e., the side to which the ink is applied), and the side where the coating with a smaller dry coating amount is arranged is the B side (i.e., the side to which the post-treatment liquid is applied). Furthermore, when the coating is arranged only on one side of the pulp layer, the side where the coating is arranged is the A side (i.e., the side to which the ink is applied), and the side where the coating is not arranged is the B side (i.e., the side to which the post-treatment liquid is applied).

[0069] In the inkjet recording method of the present invention, since the dry coating amount of the coating layer disposed on the B side is 10 g / m 2 Therefore, the post-processing liquid can easily penetrate and the generation of cracks when the image recorded material is bent can be suppressed.

[0070] From the viewpoint of the vividness of the finished product of the image recorded material, the dry coating weight of the coating layer disposed on the A side is preferably 15 g / m2 ~40g / m 2 , more preferably 15g / m 2 ~30g / m 2 .

[0071] From the viewpoint of suppressing cracks during bending, the dry coating amount of the coating layer disposed on the B side is preferably 7 g / m 2 Below, more preferably 4g / m 2 The dry coating amount of the coating layer disposed on the B side can be 0 g / m 2 The dry coating weight of the coating layer disposed on the B side is 0 g / m 2 This means that a coating is disposed on only one side of the pulp layer.

[0072] The coating layer comprises at least one white pigment selected from the group consisting of calcium carbonate and kaolin, and a binder.

[0073] The type of the binder contained in the coating layer is not particularly limited, and examples thereof include starch, styrene-butadiene copolymer, acrylic resin, polyvinyl acetate, and polyvinyl alcohol.

[0074] The content of the white pigment is not particularly limited, and is, for example, 50% by mass to 95% by mass based on the total amount of the coating layer.

[0075] The content of the binder is not particularly limited, and is, for example, 5% by mass to 50% by mass relative to the total amount of the coating layer.

[0076] The basis weight of the paper substrate is not particularly limited, but is preferably 180 g / m 2 ~600g / m 2 , more preferably 250g / m 2 ~400g / m 2 .

[0077] Generally, the greater the basis weight of the paper substrate, the greater the thickness. The thickness of the paper substrate is not particularly limited, but is preferably 150 μm to 750 μm, more preferably 200 μm to 500 μm. The thicker the paper substrate, the more likely it is to crack when the image recorded material is bent. According to the inkjet recording method involved in the present invention, even if the basis weight of the paper substrate is within the above range, that is, even if the thickness of the paper substrate is thick, the generation of cracks can be suppressed when the image recorded material is bent.

[0078] Basis weight refers to the weight per 1m 2 Mass of paper substrate: Basis weight is measured by the method described in JIS P8124:2011.

[0079] As the paper substrate, commercially available products can be used. Examples of commercially available products include "OK Ball", "UF Coat", and "NEW Pigeon" manufactured by Ojimateria Co., Ltd.; "NEW Ultra H", "Be Light Card", "NEW Refine", "JET Ace", "JET STAR F", and "FroshWhite Card SF" manufactured by NIPPON PAPER INDUSTRIES CO., LTD.; "NEW Tough Ivory", "High Clean Coat", "NEW Clean Coat V", "NEW-DV-F", and "Maricoat-F" manufactured by Hokuetsu Corporation; "Crescendo", "TANGO", "Reliant Coated Cover", and "Carolina Coated Cover" manufactured by WestRock Company; "UPM UniquePack" and "UPM FlexPack" manufactured by UPM Specialty Papers; and "CrownBoard" and "Liquid FC" manufactured by BillerudKorsnas.

[0080] <Ink application process>

[0081] The inkjet recording method according to the present invention includes a step of applying ink containing a colorant and water to surface A, which is one surface of a paper substrate, by an inkjet recording method (hereinafter also referred to as “ink applying step”).

[0082] (Ink)

[0083] The ink applied in the ink applying step contains water.

[0084] The water content is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more relative to the total amount of the ink. The upper limit of the water content is not particularly limited, but is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.

[0085] The ink applied in the ink applying step includes at least one colorant.

[0086] Examples of the colorant include dyes and pigments, of which the colorant is preferably a pigment from the viewpoint of durability such as heat resistance, light resistance, and water resistance.

[0087] When a pigment is used as a colorant, the pigment can be included in the ink as a pigment dispersion. The pigment dispersion is a liquid obtained by dispersing the pigment in a liquid medium using a pigment dispersant, and contains at least a pigment, a dispersant, and a liquid medium. The details of the dispersant will be described later. In addition, the liquid medium can be water or an organic solvent.

[0088] The pigment may be an organic pigment or an inorganic pigment.

[0089] Examples of the organic pigment include azo pigments, polycyclic pigments, dye chelates, nitro pigments, nitroso pigments, and aniline black. Among them, the organic pigment is preferably an azo pigment or a polycyclic pigment.

[0090] Examples of the azo pigment include azo lakes, insoluble azo pigments, condensed azo pigments, and chelated azo pigments.

[0091] Examples of the polycyclic pigment include phthalocyanine pigments, perylene pigments, perylone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments.

[0092] Examples of the dye chelate include basic dye type chelates and acid dye type chelates.

[0093] Examples of the inorganic pigment include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, and carbon black.

[0094] Examples of the pigment include pigments described in "Encyclopedia of Pigments" edited by Seijiro Ito (published in 2000), "Industrial Organic Pigments" by W. Herbst, K. Hunger, JP-A-2002-12607, JP-A-2002-188025, JP-A-2003-26978, and JP-A-2003-342503.

[0095] In the ink, the volume average particle size of the pigment is preferably 10 nm to 200 nm, more preferably 20 nm to 180 nm, and further preferably 30 nm to 150 nm. If the volume average particle size is 200 nm or less, the color reproducibility becomes good, and the ejection property is improved when recording an image by an inkjet recording method. In addition, if the volume average particle size is 10 nm or more, the light resistance becomes good.

[0096] Furthermore, the particle size distribution of the pigment is not particularly limited, and may be either a broad particle size distribution or a monodisperse particle size distribution. Furthermore, two or more pigments having a monodisperse particle size distribution may be mixed and used.

[0097] The volume average particle size and particle size distribution of the pigment are values ​​measured by a particle size distribution measuring device (for example, Microtrac UPA (registered trademark) EX150 manufactured by Nikkiso Co., Ltd.).

[0098] The content of the colorant is preferably 1% by mass to 20% by mass, and more preferably 1% by mass to 10% by mass, based on the total amount of the ink.

[0099] When the ink imparted in the ink imparting process contains a pigment, in order to disperse the pigment in water, the ink preferably contains a pigment dispersant. In the present invention, a pigment dispersant refers to a compound having a function of dispersing a pigment. The pigment can be dispersed in water by adsorbing the pigment dispersant to the surface of the pigment and covering at least a portion of the surface of the pigment. In addition, as a pigment, when a self-dispersible pigment that can be dispersed in water without a pigment dispersant is used, the ink may not contain a pigment dispersant.

[0100] The form of the pigment dispersant contained in the ink is not particularly limited, and can be any one of a random polymer, a block polymer, and a graft polymer. In addition, the pigment dispersant can be a polymer having a cross-linked structure. Among them, the pigment dispersant is preferably a polymer having a cross-linked structure. If the pigment dispersant is a polymer having a cross-linked structure, it is believed that the pigment dispersant is not easy to detach from the surface of the pigment, and the dispersion stability of the pigment is high.

[0101] In the present invention, the polymer refers to a compound having a weight average molecular weight of 1,000 or more.

[0102] In the present invention, the weight average molecular weight refers to the value obtained by gel permeation chromatography (GPC). When measuring by gel permeation chromatography (GPC), HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation) is used as a measuring device, 3 TSKgel (registered trademark) Super Multipore HZ-H (4.6 mmID×15 cm, manufactured by Tosoh Corporation) are used as a column, and THF (tetrahydrofuran) is used as an eluent. In addition, an RI detector is used for measurement, wherein the sample concentration is set to 0.45% by mass, the flow rate is set to 0.35 ml / min, the sample injection amount is set to 10 μl, and the measurement temperature is set to 40°C. The calibration curve was prepared using eight samples of "standard sample TSK standard, polystyrene (polystyrene)" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000" and "n-propylbenzene".

[0103] From the viewpoint of dispersion stability, the content of the dispersant in the ink is preferably 0.5 to 3.0, more preferably 1.0 to 2.0, based on mass, relative to the content of the pigment.

[0104] From the viewpoint of improving ejection properties, the ink applied in the ink applying step preferably contains at least one organic solvent.

[0105] Examples of the organic solvent include glycerin, 1,2,6-hexanetriol, trimethylolpropane, polyols such as alkanediol (e.g., ethylene glycol, 1,2-propylene glycol), 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, 1,2-octanediol, 1,2-hexanediol, 1,2-pentanediol, 4-methyl-1,2-pentanediol, etc.), polyalkylene glycol (e.g., diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, dipropylene glycol, polyoxyethylene polyoxypropylene glycol, etc.);

[0106] Polyalkylene glycol ethers (e.g., diethylene glycol monoalkyl ether, triethylene glycol monoalkyl ethyl ether, tripropylene glycol monoalkyl ethyl ether, polyoxypropylene glycerol ether, etc.);

[0107] Alkyl alcohol having 1 to 4 carbon atoms, 2-pyrrolidone, and N-methyl-2-pyrrolidone.

[0108] The content of the organic solvent is preferably 0.5% by mass to 30% by mass, more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 15% by mass, based on the total amount of the ink.

[0109] From the viewpoint of improving ejection properties, the ink applied in the ink applying step preferably contains at least one water-soluble resin.

[0110] In the present invention, the "water-soluble" in the water-soluble resin means a property that the amount of the water-soluble resin dissolved in 100 g of water at 25°C is 1 g or more.

[0111] The water-soluble resin is preferably a water-soluble resin X1 containing an alkyl group having 1 to 3 carbon atoms, an anionic group, and a cyclic structure.

[0112] When the water-soluble resin includes the water-soluble resin X1, the proportion of the water-soluble resin X1 in the total amount of the water-soluble resin is preferably 50 to 100% by mass, more preferably 60 to 100% by mass, and further preferably 80 to 100% by mass.

[0113] The alkyl group having 1 to 3 carbon atoms in the water-soluble resin X1 is a methyl group, an ethyl group or a propyl group (ie, a n-propyl group or an isopropyl group), preferably a methyl group or an ethyl group, and more preferably a methyl group.

[0114] The water-soluble resin X1 may contain only one type of alkyl group having 1 to 3 carbon atoms, or may contain two or more types.

[0115] The alkyl group having 1 to 3 carbon atoms in the water-soluble resin X1 can be introduced into the structure of the water-soluble resin X1 by polymerizing a polymerizable monomer containing an alkyl group having 1 to 3 carbon atoms.

[0116] That is, the water-soluble resin X1 may include a structural unit derived from a polymerizable monomer including an alkyl group having 1 to 3 carbon atoms.

[0117] The polymerizable monomer containing an alkyl group having 1 to 3 carbon atoms is preferably an alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms in the alkyl ester structure (hereinafter also referred to as "C1-3 alkyl (meth)acrylate").

[0118] Specifically, the C1-3 alkyl (meth)acrylate is methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate or isopropyl (meth)acrylate.

[0119] As the C1-3 alkyl (meth)acrylate, methyl (meth)acrylate or ethyl (meth)acrylate is preferred, and methyl (meth)acrylate is more preferred.

[0120] Furthermore, as the (meth)acrylic acid C1-3 alkyl ester, methacrylate C1-3 alkyl ester is preferred.

[0121] When the water-soluble resin X1 contains a C1-3 alkyl (meth)acrylate unit, the C1-3 alkyl (meth)acrylate unit in the water-soluble resin X1 may be of only one type or of two or more types.

[0122] The content of the C1-3 alkyl (meth)acrylate unit in the water-soluble resin X1 is preferably 3 to 80% by mass, more preferably 3 to 50% by mass, and even more preferably 5 to 50% by mass, based on the total amount of the water-soluble resin X1.

[0123] -Anionic Group-

[0124] Examples of the anionic group in the water-soluble resin X1 include acid groups (eg, carboxyl groups, sulfonyl groups, phosphoric acid groups, etc.) and salts of acid groups (eg, carboxyl group salts, sulfonyl group salts, phosphoric acid group salts).

[0125] The anionic group contained in the water-soluble resin X1 may be only one kind or two or more kinds.

[0126] The water-soluble resin X1 may contain both an acid group and a salt of an acid group as an anionic group.

[0127] The salt of an acid group (eg, a salt of a carboxyl group, a salt of a sulfonic group, and a salt of a phosphoric acid group) can be formed by neutralizing the acid group (eg, a carboxyl group, a sulfonic group, and a phosphoric acid group) with a neutralizing agent.

[0128] Neutralization of the acid group may be performed before polymerizing the polymerizable monomer containing an acid group, or may be performed after polymerizing the polymerizable monomer.

[0129] Examples of the neutralizing agent for neutralizing the acid group include inorganic bases such as alkali metal hydroxides and alkaline earth metal hydroxides and organic bases such as organic amines.

[0130] Examples of the alkali metal include potassium (K) and sodium (Na).

[0131] Examples of the alkaline earth metal include calcium (Ca) and magnesium (Mg).

[0132] Examples of the alkali metal hydroxide include potassium hydroxide and sodium hydroxide.

[0133] Examples of the hydroxide of the alkaline earth metal include calcium hydroxide and magnesium hydroxide.

[0134] Examples of the organic amine include ammonia, primary amines (e.g., ethylamine, monoethanolamine, etc.), secondary amines (e.g., diethylamine, ethylenediamine, etc.), tertiary amines (e.g., triethylamine, triethanolamine, isopropylethylamine, pyrrolidine, piperidine, etc.), and quaternary ammonium salts. Among them, the organic amine is preferably an organic amine having a boiling point of 80° C. or higher from the viewpoint of storage stability.

[0135] From the viewpoint of storage stability, the neutralizing agent is preferably an alkali metal hydroxide or an organic amine, and more preferably an alkali metal hydroxide or an organic amine having a boiling point of 80° C. or higher.

[0136] Examples of organic amines having a boiling point of 80° C. or higher include ethylenediamine (117° C.), triethylamine (90° C.), monoethanolamine (170° C.), triethanolamine (208° C.), isopropylethylamine (127° C.), pyrrolidine (87° C.), and piperidine (106° C.).

[0137] The water-soluble resin X1 preferably contains at least one of a carboxyl group and a salt of a carboxyl group as an anionic group.

[0138] In this case, the ratio of the salt of the carboxyl group to the total of the carboxyl group and the salt of the carboxyl group (mol %; hereinafter also referred to as the degree of neutralization) is preferably 40 mol % or more, preferably 50 mol % or more, more preferably 60 mol % or more, and further preferably 80 mol % or more.

[0139] Furthermore, the upper limit of the degree of neutralization can be set to 100 mol %.

[0140] The anionic group that may be contained in the water-soluble resin X1 can be introduced into the structure of the water-soluble resin X1 by polymerizing a polymerizable monomer containing anionic groups (and, if necessary, neutralizing it using a neutralizing agent).

[0141] That is, the water-soluble resin X1 may include a structural unit derived from a polymerizable monomer including an anionic group.

[0142] As the polymerizable monomer containing an anionic group, (meth)acrylic acid is particularly preferred.

[0143] When the water-soluble resin X1 contains a structural unit derived from a polymerizable monomer containing an anionic group (for example, (meth)acrylic acid), the content of the structural unit derived from the polymerizable monomer containing anionic group is preferably 5% by mass to 40% by mass, and more preferably 8% by mass to 20% by mass, based on the total amount of the water-soluble resin X1.

[0144] The cyclic structure in the water-soluble resin X1 preferably includes at least one of an aromatic ring and an aliphatic ring, and more preferably includes an aromatic ring.

[0145] The water-soluble resin X1 may contain only one type of cyclic structure, or may contain two or more types.

[0146] In the present invention, the aromatic ring refers to a cyclic unsaturated ring having aromaticity.

[0147] Examples of the aromatic ring include:

[0148] Aromatic hydrocarbon rings such as benzene ring, naphthalene ring, anthracene ring, pyrene ring, etc.; and

[0149] Heteroaromatic rings such as pyridine ring, pyrrole ring, furan ring, thiophene ring, imidazole ring and acridone ring.

[0150] Among them, the aromatic ring is preferably an aromatic hydrocarbon ring.

[0151] When the cyclic structure in the water-soluble resin X1 includes an aromatic ring, the aromatic ring can be introduced into the structure of the water-soluble resin X1 by polymerizing a polymerizable monomer including an aromatic ring.

[0152] As the polymerizable monomer containing an aromatic ring, a polymerizable monomer containing an aromatic ring and an ethylenically unsaturated double bond is preferred, and a vinyl polymerizable monomer containing an aromatic ring is more preferred.

[0153] Examples of the polymerizable monomer containing an aromatic ring include styrene, methylstyrene, divinylbenzene, vinylpyridine, diallyl phthalate, and (meth)acrylate containing an aromatic ring (for example, benzyl acrylate, phenoxyethyl acrylate, etc.).

[0154] The polymerizable monomer containing an aromatic ring may be unsubstituted or substituted with a substituent. Examples of the substituent include a halogen atom, an alkyl group, a carboxylic acid group, and a hydroxyl group.

[0155] Examples of the halogen atom include a chlorine atom, a bromine atom and an iodine atom.

[0156] The alkyl group is preferably an alkyl group having 1 to 12 carbon atoms (preferably 1 to 8 carbon atoms), and examples thereof include methyl, ethyl, propyl, butyl, and hexyl. The alkyl group may be unsubstituted or may have the same substituents as described above.

[0157] Specific examples of the structural unit derived from the polymerizable monomer containing an aromatic ring which may be contained in the water-soluble resin X1 are the same as the specific examples of the structural unit derived from the polymerizable monomer containing an aromatic ring which may be contained in the above-mentioned pigment dispersion resin.

[0158] The content of the structural unit derived from the polymerizable monomer containing a cyclic structure (eg, aromatic ring) in the water-soluble resin X1 is preferably 50 to 85% by mass, more preferably 60 to 80% by mass, based on the total amount of the water-soluble resin X1.

[0159] The water-soluble resin X1 particularly preferably contains a structural unit derived from a C1-3 alkyl (meth)acrylate (i.e., a (meth)acrylate alkyl ester in which the alkyl group in the alkyl ester structure has 1 to 3 carbon atoms), a structural unit derived from (meth)acrylic acid, and a structural unit derived from a polymerizable monomer containing a cyclic structure.

[0160] Preferred contents of the respective structural units in this embodiment are as described above.

[0161] In the above embodiment, the concept of "structural unit derived from (meth)acrylic acid" includes both structural units obtained by polymerization of (meth)acrylic acid (i.e., structural units containing a carboxyl group) and structural units obtained by polymerization and neutralization of (meth)acrylic acid (i.e., structural units containing a salt of a carboxyl group) (here, neutralization may be performed before or after polymerization).

[0162] The weight average molecular weight of the water-soluble resin X1 is preferably 5,000 to 100,000. When the weight average molecular weight of the water-soluble resin X1 is within the above range, bleeding and blocking of the image can be further suppressed, and the ink ejection property can be further improved.

[0163] The weight average molecular weight of the water-soluble resin X1 is more preferably 10,000 to 80,000, and even more preferably 10,000 to 30,000, from the viewpoint of ink ejection properties.

[0164] The ink applied in the ink application step preferably contains a surfactant. The type of the surfactant is not particularly limited, and may be any of anionic surfactants, cationic surfactants, betaine surfactants, and nonionic surfactants.

[0165] The content of the surfactant is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass, based on the total amount of the ink.

[0166] The ink applied in the ink application step may contain additives such as wax, colloidal silica, a defoaming agent, a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, and a basic compound as needed.

[0167] The surface tension of the ink applied in the ink applying step is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and further preferably 25 mN / m to 45 mN / m.

[0168] The surface tension of the ink is measured at a temperature of 25° C. using a surface tensiometer, for example, an automatic surface tensiometer manufactured by Kyowa Interface Science Co., Ltd. (product name “DY-300”).

[0169] The viscosity of the ink applied in the ink applying step is preferably 1.2 mPa·s to 15.0 mPa·s, more preferably 2.0 mPa·s to 13.0 mPa·s or less, and even more preferably 2.5 mPa·s to 10.0 mPa·s or less.

[0170] The viscosity of the ink is measured at a temperature of 30° C. using a rotational viscometer, for example, product name “VISCOMETER TV-22” manufactured by Toki Sangyo Co., Ltd.

[0171] From the viewpoint of storage stability of the ink, the pH of the ink applied in the ink applying step is preferably 6.0 to 11.0, more preferably 7.0 to 10.0, and even more preferably 7.0 to 9.0.

[0172] The pH of the ink is measured at a temperature of 25° C. using a pH meter, for example, a product name “WM-50EG” manufactured by DKK-TOA CORPORATION.

[0173] (Inkjet recording method)

[0174] The inkjet recording method is not particularly limited as long as it can record an image, and a known method can be used. Examples of the inkjet recording method include a charge control method that uses electrostatic induction force to eject ink, a drop-on-demand method (pressure pulse method) that uses vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electrical signal into an acoustic beam and irradiates the ink to eject the ink using radiation pressure, and a thermal inkjet (bubble jet (registered trademark)) method that heats the ink to form bubbles and uses the generated pressure.

[0175] Examples of inkjet heads used in the inkjet recording method include a shuttle method in which a short-sized serial head is used to scan the head in the width direction of the substrate and perform recording, and a line method in which a line head is used in which recording elements are arranged over the entire area corresponding to one side of the substrate.

[0176] In the inline method, by scanning the substrate in a direction intersecting the arrangement direction of the recording elements, a pattern can be formed on the entire surface of the substrate, and a transport system such as a carriage for scanning a short-sized nozzle is not required. In addition, in the inline method, only the substrate is moved without the need for complex scanning control of the carriage and the substrate, so the recording speed can be increased compared to the reciprocating method.

[0177] The ejection amount of the ink ejected from the inkjet head is preferably 1 pL (picoliter) to 100 pL, more preferably 1 pL to 10 pL, and even more preferably 1 pL to 5 pL.

[0178] <Infrared irradiation process>

[0179] The inkjet recording method according to the present invention includes a step of irradiating the surface A provided with ink with infrared rays having a maximum wavelength in the range of 800 nm to 3,000 nm (hereinafter also referred to as “infrared irradiation step”).

[0180] The ink applied in the ink applying step is dried by irradiating with infrared rays.

[0181] The maximum wavelength in infrared light refers to the wavelength at which the radiation energy density reaches the maximum. The maximum wavelength is calculated according to the temperature of the radiator and the "Planck radiation law". For example, when the radiator is a filament, the maximum wavelength at a filament temperature of 1,200°C is 2,415nm, and at 3,500°C it is 828nm.

[0182] From the viewpoint of improving the scratch resistance of an image, the infrared ray is preferably a near infrared ray having a maximum wavelength in the range of 800 nm to 1,400 nm.

[0183] The irradiation energy of infrared rays is not particularly limited, but is preferably 50 kJ / m from the viewpoint of drying properties. 2 ~500kJ / m 2 , more preferably 60 kJ / m 2 ~400kJ / m 2 , especially preferably 70 kJ / m 2 ~300kJ / m 2 .

[0184] The infrared irradiation method is not particularly limited, and for example, a common infrared lamp, a xenon flash lamp, a xenon lamp, a xenon short arc lamp, a near-infrared halogen heater, an infrared LED, an infrared laser, or the like can be used for irradiation.

[0185] <Post-treatment liquid application step>

[0186] The inkjet recording method according to the present invention includes a step of applying a post-treatment liquid containing water and a surfactant to the other side B of the paper substrate (hereinafter also referred to as a “post-treatment liquid applying step”).

[0187] The post-treatment liquid applied in the post-treatment liquid applying step contains water.

[0188] The water content is preferably 90% by mass or more, more preferably 95% by mass or more, and further preferably 98% by mass or more relative to the total amount of the post-treatment liquid. The upper limit of the water content is not particularly limited, and is, for example, 99.95% by mass.

[0189] The post-treatment liquid applied in the post-treatment liquid applying step contains at least one surfactant.

[0190] The type of surfactant is not particularly limited, and may be any of anionic surfactants, cationic surfactants, betaine surfactants, and nonionic surfactants.

[0191] Examples of the anionic surfactant include fatty acid salts, alkyl sulfate ester salts, alkylbenzene sulfonates, alkylnaphthalene sulfonates, dialkyl sulfosuccinates, alkyl phosphate ester salts, naphthalenesulfonic acid formalin condensates, and polyoxyethylene alkyl sulfate ester salts.

[0192] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkylpyridinium salts, alkylquaternary ammonium salts, alkyldimethylbenzylammonium salts, alkylisoquinolinium salts, dialkylmorpholinium salts, polyoxyethylenealkylamines, alkylamine salts, polyamine fatty acid derivatives, amyl alcohol fatty acid derivatives, benzalkonium chloride, and benzethonium chloride.

[0193] Examples of the betaine-based surfactants include coconut oil alkyl dimethylamine oxide and fatty acid amide propyl dimethylamine oxide.

[0194] Examples of the nonionic surfactant include polyoxyethylene higher alkyl ethers, polyoxyethylene higher alkylphenyl ethers, higher fatty acid diesters of polyoxyethylene glycol, acetylene glycol-based surfactants, silicone-based surfactants, and fluorine-based surfactants.

[0195] Among them, the surfactant is preferably a nonionic surfactant. If the post-treatment liquid contains a nonionic surfactant, the post-treatment liquid easily penetrates into the B surface of the paper substrate, so the effect of suppressing the generation of cracks when the image recorded material is bent is high.

[0196] Furthermore, the HLB (Hydrophile-Lipophile Balance) value of the surfactant is preferably 8.0 to 14.0, and more preferably 9.0 to 13.0. When the HLB value of the surfactant is within the above range, the post-treatment liquid easily penetrates into the B surface of the paper substrate, thereby having a high effect of suppressing the generation of cracks when the image recorded material is bent.

[0197] When the post-treatment liquid contains two or more surfactants, it is preferable that the weighted average value of the HLB values ​​of the respective surfactants is within the above range.

[0198] The HLB value is calculated by the following Kawakami formula.

[0199] HLB=7+11.7log(Mw / Mo)

[0200] Here, Mw is the molecular weight of the hydrophilic group, and Mo is the molecular weight of the hydrophobic group.

[0201] In the present invention, regarding the HLB value, when a catalog value can be confirmed, the catalog value is preferably adopted.

[0202] The post-treatment liquid applied in the post-treatment liquid application step may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, a conductive salt, and a basic compound, as necessary.

[0203] The surface tension of the post-treatment liquid applied in the post-treatment liquid application step is preferably 20.0 mN / m to 45.0 mN / m, more preferably 22.5 mN / m to 40.0 mN / m, and further preferably 25.0 mN / m to 35.0 mN / m. The surface tension of the post-treatment liquid is measured in the same manner as the surface tension of the ink.

[0204] When the surface tension of the post-treatment liquid is within the above range, the post-treatment liquid easily permeates the B surface of the paper substrate, and thus the effect of suppressing the occurrence of cracks when the image recorded material is bent is high.

[0205] The method for applying the post-treatment liquid is not particularly limited, and examples thereof include known methods such as a coating method, a dipping method, a flexographic printing method, and an inkjet recording method.

[0206] The amount of the post-treatment liquid applied per unit area is preferably 3 g / m 2 ~70g / m 2 , more preferably 10g / m 2 ~55g / m 2 If the amount applied is 3g / m 2 On the other hand, if the amount of the applied film is 70 g / m 2If the breaking strength of the image recorded material is high, the image recorded material can be prevented from being broken in the device.

[0207] In the inkjet recording method of the present invention, the post-treatment liquid is allowed to permeate into the paper substrate to suppress the occurrence of cracks when the image recorded material is folded. Therefore, it is preferred not to provide a step of heating and drying the post-treatment liquid after the step of applying the post-treatment liquid.

[0208] <Pre-treatment liquid application step>

[0209] From the viewpoint of improving the abrasion resistance of the image, the inkjet recording method of the present invention preferably includes a step of applying a pretreatment liquid to surface A before the ink applying step (hereinafter also referred to as a "pretreatment liquid applying step"). When the pretreatment liquid applying step is included, in the ink applying step, ink is applied to surface A to which the pretreatment liquid is applied.

[0210] The pretreatment liquid applied in the pretreatment liquid application step preferably contains a coagulant. The coagulant is not particularly limited as long as it is a component that causes the components in the ink to coagulate. The coagulant is preferably at least one selected from the group consisting of a polyvalent metal compound, an organic acid, a metal complex, and a cationic polymer, and more preferably contains an organic acid.

[0211] -Multivalent Metal Compounds-

[0212] Examples of polyvalent metal compounds include salts of alkaline earth metals of Group 2 of the periodic table (e.g., magnesium and calcium), transition metals of Group 3 of the periodic table (e.g., lanthanum), metals of Group 13 of the periodic table (e.g., aluminum), and lanthanides (e.g., neodymium).

[0213] The salt of these metals is preferably a salt of an organic acid described later, a nitrate, a chloride or a thiocyanate.

[0214] Among them, the polyvalent metal compound is preferably a calcium salt or a magnesium salt of an organic acid (eg, formic acid, acetic acid, benzoic acid, etc.); a calcium salt or a magnesium salt of nitrate; calcium chloride, magnesium chloride, or a calcium salt or a magnesium salt of thiocyanate.

[0215] It is preferred that at least a part of the polyvalent metal compound is dissociated into polyvalent metal ions and counter ions in the pretreatment liquid.

[0216] -Organic Acids-

[0217] Examples of the organic acid include organic compounds having an acidic group.

[0218] Examples of the acidic group include a phosphoric acid group, a phosphonic acid group, a phosphinic acid group, a sulfuric acid group, a sulfonic acid group, a sulfonic acid group, a sulfinic acid group, and a carboxyl group.

[0219] Among them, from the viewpoint of the aggregation speed of the ink, the acidic group is preferably a phosphoric acid group or a carboxyl group, and more preferably a carboxyl group.

[0220] It is preferred that at least a part of the acidic groups be dissociated in the pretreatment liquid.

[0221] Examples of the organic compound having a carboxyl group include (meth)acrylic acid, poly(meth)acrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidonecarboxylic acid, pyranonecarboxylic acid, pyrrolecarboxylic acid, furancarboxylic acid, pyridinecarboxylic acid, coumaric acid, thiophenecarboxylic acid and nicotinic acid.

[0222] Among them, from the viewpoint of the aggregation speed of the ink, the organic compound having a carboxyl group is preferably a divalent or higher-valent carboxylic acid (hereinafter also referred to as a polyvalent carboxylic acid), and more preferably a dicarboxylic acid.

[0223] Specifically, the polycarboxylic acid is preferably malonic acid, malic acid, maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, tartaric acid, 4-methylphthalic acid or citric acid, and more preferably malonic acid, malic acid, tartaric acid, succinic acid, glutaric acid, pimelic acid, adipic acid or citric acid.

[0224] The organic acid preferably has a low pKa (eg, 1.0 to 5.0). Thus, the surface charge of particles such as pigments and resin particles in the ink dispersed and stabilized by weakly acidic functional groups such as carboxyl groups can be reduced by contact with an organic acid with a lower pKa, thereby reducing dispersion stability.

[0225] The organic acid preferably has a low pKa, high solubility in water, and a valence of 2 or more. Furthermore, the organic acid more preferably has a high buffering capacity in a pH region lower than the pKa of the functional group (eg, carboxyl group) that stabilizes particle dispersion in the ink.

[0226] -Metal Complex-

[0227] The metal complex preferably contains at least one selected from the group consisting of zirconium, aluminum, and titanium as the metal element.

[0228] The metal complex preferably contains, as a ligand, at least one selected from the group consisting of acetate, acetylacetone, methyl acetoacetate, ethyl acetoacetate, octanediol, butoxyacetylacetone, lactate, ammonium lactate, and triethanolamine.

[0229] The metal complex can be a commercially available product. Various organic ligands, especially various multidentate ligands capable of forming metal chelate catalysts, can be purchased. Therefore, the metal complex can be a metal complex prepared by combining commercially available organic ligands and metals.

[0230] Examples of the metal complex include zirconium tetraacetylacetonate (e.g., “ORGATIX ZC-150” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoacetylacetonate (e.g., “ORGATIX ZC-540” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium diacetylacetonate (e.g., “ORGATIX ZC-550” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoethyl acetylacetonate (e.g., “ORGATIX ZC-560” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium acetate (e.g., “ORGATIX ZC-115” manufactured by Matsumoto Fine Chemical Co., Ltd.), diisopropoxybis(acetylacetonate)titanium (e.g., “ORGATIX TC-100” manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium tetraacetylacetonate (e.g., “ORGATIX ZC-550” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium monoethyl acetylacetonate (e.g., “ORGATIX ZC-560” manufactured by Matsumoto Fine Chemical Co., Ltd.), zirconium acetate (e.g., “ORGATIX ZC-115” manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium tetraacetylacetonate (e.g., “ORGATIX TC-100” manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium tetraacetylacetonate (e.g., “ORGATIX ZC-550” manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium mono ... Chemical Co., Ltd., "ORGATIX TC-401" manufactured by Matsumoto Fine Chemical Co., Ltd.), dioctyloxybis(octanediol)titanium (e.g., "ORGATIX TC-200" manufactured by Matsumoto Fine Chemical Co., Ltd.), diisopropoxybis(ethyl acetoacetate)titanium (e.g., "ORGATIX TC-750" manufactured by Matsumoto Fine Chemical Co., Ltd.), tetraacetylacetonate zirconium (e.g., "ORGATIX ZC-700" manufactured by Matsumoto Fine Chemical Co., Ltd.), tributoxymonoacetylacetonate zirconium (e.g., "ORGATIX ZC-540" manufactured by Matsumoto Fine Chemical Co., Ltd.), monobutoxyacetylacetonate bis(ethyl acetoacetate) zirconium (e.g., "ORGATIX ZC-570" manufactured by Matsumoto Fine Chemical Co., Ltd.), dibutoxybis(ethyl acetoacetate) zirconium (e.g., "ORGATIX ZC-750" manufactured by Matsumoto Fine Chemical Co., Ltd.), tetraacetylacetonate zirconium (e.g., "ORGATIX ZC-700" manufactured by Matsumoto Fine Chemical Co., Ltd.), Co., Ltd.), aluminum triacetylacetonate (e.g., "ORGATIX ZC-580" manufactured by Matsumoto Fine Chemical Co., Ltd.), ammonium titanium lactate (e.g., Matsumoto Fine Chemical Co., Ltd., Ltd.), titanium lactate (e.g., "ORGATIX TC-300" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium triethanolamine (e.g., "ORGATIX TC-400" manufactured by Matsumoto Fine Chemical Co., Ltd.), and zirconium chloride compounds (e.g., "ORGATIX ZC-126" manufactured by Matsumoto Fine Chemical Co., Ltd.). .

[0231] Among them, the metal complex is preferably titanium ammonium lactate (e.g., "ORGATIX TC-300" manufactured by Matsumoto Fine Chemical Co., Ltd.), titanium lactate (e.g., "ORGATIX TC-310, 315" manufactured by Matsumoto Fine Chemical Co., Ltd.), triethanolamine titanium (e.g., "ORGATIX TC-400" manufactured by Matsumoto Fine Chemical Co., Ltd.) or a zirconium chloride compound (e.g., "ORGATIX ZC-126" manufactured by Matsumoto Fine Chemical Co., Ltd.).

[0232] -Cationic polymer-

[0233] Furthermore, the pretreatment liquid may be in a form containing one or more cationic polymers as agglomerating components. The cationic polymer is preferably a homopolymer of a cationic monomer having a primary to tertiary amino group or a quaternary ammonium salt group, a copolymer or polycondensate of a cationic monomer and a non-cationic monomer. The cationic polymer may be used in the form of a water-soluble polymer or a water-dispersible latex particle.

[0234] Examples of the cationic polymer include polyvinyl pyridinium salts, polyalkylaminoethyl acrylates, polyalkylaminoethyl methacrylates, polyvinylimidazoles, polyethyleneimine, polybiguanide, polyguanidine, polyallylamine, and derivatives thereof.

[0235] From the viewpoint of the viscosity of the pretreatment liquid, the weight average molecular weight of the cationic polymer is preferably small. When the pretreatment liquid is imparted to the recording medium by inkjet recording, it is preferably 1,000 to 500,000, more preferably 1,500 to 200,000, and further preferably 2,000 to 100,000. If the weight average molecular weight is 1000 or more, it is advantageous from the viewpoint of agglomeration speed. If the weight average molecular weight is 500,000 or less, it is advantageous in terms of ejection reliability. However, when the pretreatment liquid is imparted to the recording medium by a method other than inkjet recording, it is not limited thereto.

[0236] The coagulant contained in the pretreatment liquid may be only one kind or two or more kinds.

[0237] The content of the coagulant is preferably 0.1 to 40% by mass, more preferably 0.1 to 30% by mass, further preferably 1 to 20% by mass, and particularly preferably 1 to 10% by mass, based on the total amount of the pretreatment liquid.

[0238] The pretreatment liquid applied in the pretreatment liquid application step preferably contains water. The content of water is not particularly limited, and is, for example, 40% by mass to 70% by mass.

[0239] The pretreatment liquid applied in the pretreatment liquid application step may include other components in addition to the coagulant and water as needed. Other components that may be contained in the pretreatment liquid include organic solvents, resin particles, surfactants, solid wetting agents, colloidal silica, inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, ultraviolet absorbers, preservatives, mildew inhibitors, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, water-soluble polymer compounds (for example, water-soluble polymer compounds described in paragraphs 0026 to 0080 of Japanese Patent Application No. 2013-001854) and other well-known additives.

[0240] From the viewpoint of the aggregation speed of the ink, the pH of the pretreatment liquid is preferably 0.1 to 4.5, and more preferably 0.2 to 4.0. The method for measuring the pH of the pretreatment liquid is the same as the method for measuring the pH of the ink.

[0241] From the viewpoint of the aggregation speed of the ink, the viscosity of the pretreatment liquid is preferably 0.5 mPa·s to 10 mPa·s, and more preferably 1 mPa·s to 5 mPa·s. The viscosity is a value measured at 25° C. using a viscometer. The method for measuring the viscosity of the pretreatment liquid is the same as the method for measuring the viscosity of the ink.

[0242] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and further preferably 30 mN / m to 45 mN / m. The surface tension of the pretreatment liquid is measured in the same manner as the surface tension of the ink.

[0243] The method for applying the pretreatment liquid is not particularly limited, and examples thereof include known methods such as a coating method, a dipping method, and an inkjet recording method.

[0244] Examples of the coating method include known coating methods using a bar coater, an extrusion die coater, an air knife coater, a blade coater, a rod coater, a knife coater, an extrusion coater, a reverse roll coater, and the like.

[0245] The pretreatment liquid applied to the paper substrate may be dried by heating after the pretreatment liquid is applied. Examples of the mechanism for drying the pretreatment liquid by heating include a known heating mechanism such as a heater, a known air supply mechanism such as a dryer, and a combination of these.

[0246] Examples of methods for heating and drying the pretreatment liquid include a method of heating the paper substrate from the side opposite to the side to which the pretreatment liquid is applied by a heater, a method of blowing warm air or hot air to the side to which the pretreatment liquid is applied by the paper substrate, a method of heating the paper substrate from the side to which the pretreatment liquid is applied or from the side opposite to the side to which the pretreatment liquid is applied by an infrared heater, and a method of combining a plurality of these methods.

[0247] The heating temperature during heat drying of the pretreatment liquid is preferably 35° C. or higher, more preferably 40° C. or higher. The upper limit of the heating temperature is not particularly limited, and is, for example, 120° C.

[0248] The heating drying time is not particularly limited, but is preferably 0.5 to 60 seconds, more preferably 0.5 to 20 seconds, and even more preferably 0.5 to 10 seconds.

[0249] Example

[0250] Hereinafter, embodiments of the present invention will be described in detail by way of examples, but the present disclosure is not limited thereto.

[0251] [Preparation of ink]

[0252] The components listed in Table 1 were mixed to the contents (mass %) listed in Table 1. Then, coarse particles were removed using a 1 μm filter to obtain cyan ink C1, magenta ink M1, yellow ink Y1, and black ink K1. The average particle size of the pigment in each ink, pH, viscosity, surface tension, and conductivity are shown in Table 1.

[0253] The details of each component described in Table 1 are as follows.

[0254] Cyan pigment dispersion: Product name: "Pro-jet Cyan APD1000", manufactured by FUJIFILM Imaging Colorants, pigment concentration: 14.0 mass %

[0255] Magenta pigment dispersion: product name "Pro-jet Magenta APD1000", manufactured by FUJIFILM Imaging Colorants, Inc., pigment concentration 14.0 mass %

[0256] Yellow pigment dispersion: product name "Pro-jet Yellow TP APD1000", manufactured by FUJIFILM Imaging Colorants, Inc., pigment concentration 15.4 mass%

[0257] Black pigment dispersion: product name "Pro-jet Black APD1000", manufactured by FUJIFILM Imaging Colorants, Inc., pigment concentration 14.0 mass %

[0258] · Aqueous solution of water-soluble resin PL-1: Aqueous solution of water-soluble resin prepared by the following method

[0259] 1,2-Propanediol

[0260] ·Acetylene glycol surfactant: Product name: "OLFINE E1020", manufactured by Nissin Chemical Industry Co., Ltd.

[0261] PEG6000: Product name "Polyethylene glycol 6000", manufactured by FUJIFILM Wako Pure Chemical Corporation

[0262] · Aqueous dispersion of ester wax: product name "Cellosol 524", manufactured by CHUKYO YUSHI CO., LTD., solid content concentration 30 mass%

[0263] · Aqueous dispersion of colloidal silica: product name "SNOWTEX XS", manufactured by Nissan Chemical Industries, Ltd., solid content concentration 20 mass %

[0264] · Defoamer: Product name "BYK-024", manufactured by BYK JAPAN KK

[0265] <Preparation of aqueous solution of water-soluble resin PL-1>

[0266] 1,2-propylene glycol (35 g) was added to a 500 ml three-necked flask equipped with a stirrer, a thermometer, a reflux cooling tube, and a nitrogen inlet tube, and the temperature was raised to 90°C under a nitrogen flow. A mixed solution obtained by mixing 5.55 g of dimethyl-2,2'-azobis(2-methylpropionate) (product name "V-601", manufactured by FUJIFILM Wako Pure Chemical Corporation) as a polymerization initiator, 10.7 g of methacrylic acid (MAA), 69.3 g of methyl methacrylate (MMA), 20.0 g of isobornyl methacrylate (IBOMA), 1.63 g of dodecyl mercaptan, and 65.00 g of 1,2-propylene glycol was added dropwise at a constant rate over 2 hours. After the addition of the mixed solution was completed, it was stirred for 1 hour. Next, a mixed solution obtained by mixing 1.85 g of V-601 and 24.62 g of 1,2-propylene glycol was added to the obtained reaction mixture, and the mixture was further stirred for 1.5 hours. After 120.21 g of 1,2-propylene glycol was added to the obtained reaction mixture, 8.56 g of a 50% by mass sodium hydroxide aqueous solution was added dropwise using a dropping funnel to obtain an aqueous solution of a water-soluble resin PL-1 (solid content concentration: 30% by mass).

[0267] The water-soluble resin PL-1 [MAA / MMA / IBOMA] had an acid value of 60 mgKOH / g and a weight average molecular weight (Mw) of 15,000.

[0268] [Table 1]

[0269] C1 M1 Y1 K1 Cyan pigment dispersion 21.10 - - 3.40 Magenta Pigment Dispersion - 51.00 - 5.00 Yellow pigment dispersion - - 32.80 - Black pigment dispersion - - - 18.30 Aqueous solution of water-soluble resin PL-1 14.00 12.00 14.00 14.00 1,2-Propanediol 3.80 6.00 4.20 3.20 Acetylene glycol surfactant 0.90 0.90 0.90 0.90 PEG6000 0.90 0.70 0.90 0.90 Aqueous dispersion of ester wax 6.80 6.80 6.80 6.80 Colloidal silica aqueous dispersion 0.27 0.27 0.27 0.27 Defoaming agent 0.01 0.01 0.01 0.01 water 52.22 22.32 40.12 47.22 Average particle size of pigment (nm) 118 116 135 110 pH[25℃] 8.2 8.2 8.2 8.3 Viscosity (mPa·s) [30℃] 4.8 5.0 4.8 4.9 Surface tension (mN / m) [25℃] 37.0 37.1 36.7 37.3 Electrical conductivity (mS / m) [25℃] 188 192 218 183

[0270] [Preparation of pretreatment solution 1]

[0271] The following components were mixed and filtered using a 1 μm filter to obtain a pretreatment solution 1 having a pH of 4.3.

[0272] Malonic acid……10.90 mass%

[0273] ·Citric acid……13.40 mass%

[0274] ·Diethylene glycol monobutyl ether……2.00 mass%

[0275] Potassium hydroxide...7.30 mass%

[0276] Defoaming agent (product name "BYK-038", manufactured by BYK JAPAN KK) ... 0.05 mass%

[0277] Polyacrylic acid having a weight average molecular weight of 25,000 (product name "Polyacrylic acid 25,000", manufactured by FUJIFILM WakoPure Chemical Corporation) ... 0.95 mass%

[0278] · Ion exchange water……65.40 mass%

[0279] [Preparation of post-treatment solution]

[0280] The surfactants and water listed in Table 2 were mixed to the contents (mass %) listed in Table 2. Then, the mixture was filtered using a 1 μm filter to obtain post-treatment liquids PT-1 to PT-17. Table 2 shows the types, classifications, and HLB values ​​of the surfactants.

[0281] The details of the surfactants described in Table 2 are as follows.

[0282] ·Acetylene glycol surfactant 1: Product name: "OLFINE E1010", manufactured by Nissin Chemical Industry Co., Ltd.

[0283] · Acetylene glycol surfactant 2: Product name: "OLFINE E1020", manufactured by Nissin Chemical Industry Co., Ltd.

[0284] · Polyoxyethylene lauryl ether 1: Product name "EMULGEN102KG", manufactured by Kao Corporation

[0285] · Polyoxyethylene lauryl ether 2: Product name "EMULGEN103", manufactured by Kao Corporation

[0286] · Polyoxyethylene lauryl ether 3: Product name "EMULGEN105", manufactured by Kao Corporation

[0287] · Polyoxyethylene lauryl ether 4: Product name "EMULGEN108", manufactured by Kao Corporation

[0288] · Polyoxyethylene lauryl ether 5: Product name "EMULGEN109P", manufactured by Kao Corporation

[0289] · Polyoxyethylene lauryl ether 6: Product name "EMULGEN120", manufactured by Kao Corporation

[0290] · Polyoxyethylene lauryl ether 7: Product name "EMULGEN150", manufactured by Kao Corporation

[0291] ・Silicone surfactant: Product name "BYK-347", manufactured by BYK JAPAN KK

[0292] ·Alkylbenzene sulfonic acid: Product name: "PIONIN A-40", manufactured by TAKEMOTO OIL&FAT CO.,LTD

[0293] · Lauryl trimethyl ammonium chloride: Product name "PIONIN B-111", manufactured by TAKEMOTO OIL&FAT CO., LTD

[0294] Fatty acid amide propyl dimethylamine oxide: Product name "PIONIN C-151", manufactured by TAKEMOTO OIL & FATCO., LTD.

[0295] [Table 2]

[0296]

[0297] [Production of image records]

[0298] In Examples 1 to 29 and Comparative Examples 1 to 2, single-sided coated paper (product name "UF Coat", manufactured by Ojimateria Co., Ltd.) was used as the paper substrate. The basis weight of the paper substrate used in each example is as shown in Table 3. In the paper substrate, the side with the coating layer is set as "side A", and the side without the coating layer is set as "side B". The dry coating amount of the coating layer set on the side of side A is about 18 g / m 2 .

[0299] In Comparative Example 3, double-sided coated paper (product name "Bon Ivory+", manufactured by Ojimateria Co., Ltd., basis weight: 310 g / m 2 The dry coating weight of the coatings on both sides was about 18 g / m 2 .

[0300] (1) Pretreatment liquid application step

[0301] The pretreatment liquid 1 was applied to the A surface of the paper substrate using a coating bar so that the application amount was 1.5 g / m 2 . Two seconds after coating, warm air at a temperature of 100° C. and a wind speed of 15 m / sec was blown toward the coated surface from a height of 10 cm for 5 seconds to dry it. In Example 29, the pretreatment liquid application step was not performed.

[0302] (2) Ink application process

[0303] Three seconds after the pretreatment liquid was dried, black ink K1, cyan ink C1, magenta ink M1, and yellow ink Y1 were ejected in sequence by a single-pass method onto the surface (surface A) of the paper substrate coated with the pretreatment liquid 1 under the following conditions, thereby recording an image.

[0304] <Conditions>

[0305] Inkjet head: 4-color printhead, 1,200 dpi (dot per inch) / 20-inch width piezoelectric full-line printhead

[0306] Ejection volume: 1.5pL (picoliter) per pixel per color

[0307] Drive frequency: 60kHz (substrate conveying speed: 1,270mm / sec)

[0308] (3) Infrared irradiation process

[0309] Two seconds after the ink was applied to the A surface, a near infrared lamp with a maximum wavelength of 830 nm was used to irradiate the surface at 250 kJ / m 2 The irradiation energy of irradiates the A surface with near infrared rays.

[0310] In Example 24, an infrared lamp having a maximum wavelength of 2,400 nm was used instead of the near-infrared lamp.

[0311] (4) Post-treatment liquid application process

[0312] Three seconds after the near infrared or infrared ray irradiation, the post-treatment liquid described in Table 3 was applied to the B surface of the paper substrate by flexographic printing in an amount described in Table 3, thereby obtaining an image recorded material. In Comparative Example 1, the post-treatment liquid application step was not performed.

[0313] [Evaluation and measurement]

[0314] The obtained image records were used to evaluate the abrasion resistance, folding resistance, and strength. The evaluation method was as follows. The evaluation results are shown in Table 3.

[0315] <Abrasion resistance>

[0316] A friction test was performed using a Gakushin type friction tester (manufactured by Yasuda Seiki Seisakusho Ltd.).

[0317] After 30 seconds from the application of the post-treatment liquid, the image recorded object was fixed on the test piece stage.

[0318] Unused paper substrate (product name: UF Coat, unit area: 310g / m 2 , manufactured by Ojimateria co., ltd.) is fixed on the friction element so that the coating layer of the unused paper substrate faces the image-recorded surface of the image-recorded object.

[0319] The friction element was placed on the test piece and a pressure of 240 g / cm was applied from above the friction element. 2 The friction resistance was evaluated based on the scratches and peeling conditions in the image of the rubbed part. The evaluation criteria are as follows. 3 or above is a level with no practical problems.

[0320] 5: In the image of the rubbed portion, no scratches were observed at all.

[0321] 4: In the image of the rubbed portion, scratches were slightly observed.

[0322] 3: The image at the rubbed portion was slightly peeled off, and extremely fine scratches were observed.

[0323] 2: The image on the rubbed part is peeled off and scratches are obvious.

[0324] 1: The image in the rubbed portion was peeled off, and a portion of the paper substrate was exposed.

[0325] <Folding resistance>

[0326] After 30 seconds from the application of the post-treatment liquid, the image recorded material was folded 180° so that the surface with the image recorded was on the outside. After the image recorded material was restored to its original state, the folded portion was observed with the naked eye, and the folding resistance was evaluated based on the state of the cracks. The evaluation criteria are as follows. 3 or above is a level with no practical problems.

[0327] 5: No cracks were observed in the bent portion.

[0328] 4: Cracks were slightly observed in the bent portion.

[0329] 3: Slight cracks were observed at the bent portion.

[0330] 2: There are obvious cracks in the bent part.

[0331] 1: The bent part is completely cracked.

[0332] <Strength>

[0333] Ten minutes after the application of the post-treatment liquid, the breaking strength of the image recorded material was measured using a TENSILON universal testing machine (product name "FTF-1250", manufactured by ORIENTEC CO., LTD.) at 22° C. and a relative humidity of 60%.

[0334] Furthermore, the breaking strength of the paper substrate before image recording was measured by the same method.

[0335] The strength was calculated according to the following formula.

[0336] Strength (%) = (breaking strength of image record / breaking strength of paper substrate) × 100

[0337] On the other hand, if the strength is less than 50%, problems such as cracking of the image recorded material may occur in the device.

[0338] In Table 3, the type and basis weight of the paper substrate are recorded. When the pre-treatment liquid imparting process is performed, it is recorded as "Y", and when the pre-treatment liquid imparting process is not performed, it is recorded as "N". Regarding the infrared irradiation process, the type of irradiation light is recorded. Regarding the post-treatment liquid imparting process, the type, imparting amount and surface tension of the post-treatment liquid and the classification, HLB value and content of the surfactant contained in the post-treatment liquid are recorded. In addition, in Comparative Example 1, since the post-treatment liquid imparting process is not performed, "-" is recorded in the column of the post-treatment liquid imparting process. In Comparative Example 2, in the post-treatment liquid imparting process, since water is used as the post-treatment liquid, it is recorded as "—" in the column related to the surfactant contained in the post-treatment liquid.

[0339] [Table 3]

[0340]

[0341] As shown in Table 3, in Examples 1 to 29, the steps are as follows: a step of imparting ink containing a colorant and water to the A surface of the paper substrate by an inkjet recording method; a step of irradiating the A surface imparted with ink with infrared rays having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step of imparting a post-treatment liquid containing water and a surfactant to the B surface of the paper substrate, wherein the paper substrate comprises a pulp layer and a coating layer disposed on at least one surface of the pulp layer, the coating layer comprising at least one white pigment selected from the group consisting of calcium carbonate and kaolin and a binder, the coating layer is disposed on the A surface side, and the dry coating amount of the coating layer disposed on the A surface side is 15 g / m 2 ~50g / m 2 Since no coating is disposed on the B-side, the generation of cracks can be suppressed when the image recorded material is bent.

[0342] On the other hand, in Comparative Example 1, since the post-processing liquid application step was not performed, it was found that cracks were generated when the image recorded material was bent.

[0343] In Comparative Example 2, since water was used as the post-processing liquid, it was found that cracks were generated when the image recorded material was bent.

[0344] In Comparative Example 3, it can be seen that the dry coating amount of the coating layer used as the paper substrate exceeds 10 g / m 2 Double-sided coated paper, so cracks occur when the image recorded material is bent.

[0345] In Example 1, since near infrared rays were irradiated in the infrared irradiation step, it was found that compared with Example 24,

[0346] The image has excellent abrasion resistance.

[0347] In Example 1, it is found that since the surface tension of the post-treatment liquid is 22.5 mN / m or more, the effect of suppressing the generation of cracks when the image recorded material is bent is higher than that of Example 14.

[0348] In Example 1, it is found that the surface tension of the post-treatment liquid is 40.0 mN / m or less, and therefore the effect of suppressing the generation of cracks when the image recorded material is bent is higher than that of Example 5.

[0349] In Example 1, it can be seen that since the amount of the post-treatment liquid applied per unit area is set to 10 g / m 2 As described above, compared with Example 15, the effect of suppressing the occurrence of cracks when the image recorded material is bent is higher.

[0350] In Example 1, it can be seen that since the amount of the post-treatment liquid applied per unit area is set to 55 g / m 2 Therefore, compared with Example 20, the strength of the image recorded material is excellent.

[0351] In Example 1, it is found that since the surfactant includes a nonionic surfactant, the effect of suppressing the generation of cracks when the image recorded material is bent is higher than that of Examples 21 to 23.

[0352] In Examples 8 to 11, it is found that since the HLB value of the surfactant is 8.0 or more, the effect of suppressing the generation of cracks when the image recorded material is bent is higher than that in Example 7.

[0353] In Examples 8 to 11, since the HLB value of the surfactant is 14.0 or more, it is found that the effect of suppressing the generation of cracks when the image recorded material is bent is higher than that of Example 12.

[0354] In Example 1, it is found that the image has excellent abrasion resistance compared with Example 29 because the pre-treatment liquid application step is performed.

[0355] [Preparation of pretreatment solution 2]

[0356] The following components were mixed and filtered using a 1 μm filter to obtain a pretreatment liquid 2 having a pH of 7.1.

[0357] Calcium formate……4.90 mass%

[0358] Calcium lactate pentahydrate……3.80 mass%

[0359] ·OLFINE E1010……0.20 mass%

[0360] BYK-024……0.01 mass%

[0361] · Ion exchange water……91.09 mass%

[0362] [Preparation of pretreatment solution 3]

[0363] The following components were mixed and filtered using a 1 μm filter to obtain a pretreatment solution 3 having a pH of 7.4.

[0364] Calcium formate: 10.10% by mass

[0365] Calcium lactate pentahydrate……8.10 mass%

[0366] ·OLFINE E1010……0.20 mass%

[0367] BYK-024……0.01 mass%

[0368] · Ion exchange water……81.59 mass%

[0369] <Example 30, Example 31>

[0370] Image recorded materials were obtained by the same method as in Example 1 except that the pretreatment liquid 1 was changed to the pretreatment liquid 2 and the pretreatment liquid 3. Evaluation was performed by the same method as in Example 1. Table 4 shows the evaluation results.

[0371] [Table 4]

[0372]

[0373] In Examples 30 and 31, as in Example 1, the occurrence of cracks when the image recorded material was folded could be suppressed.

[0374] In addition, the disclosure of Japanese Patent Application No. 2022-048836 filed on March 24, 2022 is incorporated into this specification by reference in its entirety. Furthermore, all documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard were specifically and individually described as being incorporated by reference.

Claims

1. An inkjet recording method, comprising: A step of applying ink containing a colorant and water to one side of a paper substrate, namely side A, by an inkjet recording method; a step of irradiating the surface A provided with the ink with infrared light having a maximum wavelength in the range of 800 nm to 3,000 nm; and a step of applying a post-treatment liquid containing water and a surfactant to the other side of the paper substrate, namely, side B; The paper substrate comprises a pulp layer and a coating layer disposed on at least one surface of the pulp layer. The coating comprises at least one white pigment selected from the group consisting of calcium carbonate and kaolin and a binder, The coating layer is disposed on the A-surface side, and the dry coating amount of the coating layer disposed on the A-surface side is 15 g / m 2 ~50g / m 2 , When the coating layer is not disposed on the B surface side, or when the coating layer is disposed on the B surface side, the dry coating amount of the coating layer disposed on the B surface side is 10 g / m 2 the following.

2. The inkjet recording method according to claim 1, wherein The infrared rays are near infrared rays having a maximum wavelength in the range of 800 nm to 1,400 nm.

3. The inkjet recording method according to claim 1 or 2, wherein: The surface tension of the post-treatment liquid is 22.5 mN / m to 40.0 mN / m.

4. The inkjet recording method according to any one of claims 1 to 3, wherein In the step of applying the post-treatment liquid, the amount applied per unit area is 10 g / m 2 ~55g / m 2 The post-treatment liquid is given a range of 5. The inkjet recording method according to any one of claims 1 to 4, wherein The surfactant includes a nonionic surfactant.

6. The inkjet recording method according to any one of claims 1 to 5, wherein The HLB value of the surfactant is 8.0-14.

0.

7. The inkjet recording method according to any one of claims 1 to 6, wherein The basis weight of the paper substrate is 180 g / m 2 ~600g / m 2 .

8. The inkjet recording method according to any one of claims 1 to 7, comprising: Before applying the ink, a pre-treatment liquid is applied to the surface A. In the step of applying the ink, the ink is applied to the surface A to which the pretreatment liquid has been applied.

9. The inkjet recording method according to claim 8, wherein The pretreatment solution contains an organic acid.

Citation Information

Patent Citations

  • Image forming method

    CN103287141A

  • Ink-jet printing process, apparatus and materials

    EP0787596A1

  • Tack paper and ink-jet recording method using the same

    JP2004017635A

  • Ink set, ink-jet recording method, and recorded matter

    JP2008239951A

  • Method for manufacturing inkjet recording sheet for pigment ink

    JP2012006264A