Ethylene polymer composition and pipe comprising same

Through the combination of ethylene homopolymer and ethylene-α-olefin copolymer and Ziegler-Natta catalyst polymerization, the insufficient performance of polyethylene tubes in high pressure resistance is solved, and the ethylene-based polymer composition is realized High creep strength and moldability are suitable for high demanding water and gas pipelines.

CN118922489APending Publication Date: 2024-11-08MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029561.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the use of existing polyethylene pipes that require higher pressure resistance, especially in pipes that apply internal fluid pressure for a long time or short time, it is difficult to meet higher pressure resistance requirements, such as PE112 (MRS11.2MPa or above. And the performance of less than 12.5MPa) or PE125 (MRS 12.5MPa or higher and less than 14.0MPa).

Method used

An ethylene-based polymer composition is adopted, which consists of ethylene homopolymer and copolymer of ethylene and α-olefin with 4 or more carbon atoms, and meets specific density, fluidity, molecular weight distribution and catalyst use conditions. Ziegler-Natta-based catalyst polymerizes to form a polymer with excellent moldability and low sag properties.

Benefits of technology

It has achieved excellent long-term creep strength and moldability of ethylene polymer compositions, meets the performance of MRS11.2MPa or above in ISO 9080 and 12162, while maintaining good moldability and low sag properties, and is suitable for water pipes and Uses for gas pipelines and other purposes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054911260000231
    Figure BDA0005054911260000231
  • Figure BDA0005054911260000232
    Figure BDA0005054911260000232
Patent Text Reader

Abstract

The purpose of the present invention is to obtain an ethylene-based polymer composition suitable for a polyethylene pipe having both PE112 (MRS 11.2 MPa or more) performance requiring higher creep strength and excellent moldability and low sagging properties. The present invention pertains to an ethylene-based polymer composition characterized by comprising 40-60 mass% of an ethylene homopolymer (A) having an MFR (MFR2) in the range of 100-600 g / 10 min as measured at a temperature of 190 DEG C and a load of 2.16 kg, and 60-40 mass% of a copolymer (B) of ethylene and an alpha-olefin having 4 or more carbon atoms [ethylene-alpha-olefin copolymer (B)] (provided that the total amount of (A) + (B) is 100 mass%), and the following requirements (i)-(iii) are satisfied. (i) The density is in the range of 940-960 kg / m3. (ii) The amount of components having logM > = 7 as determined by GPC is in the range of 0.35-0.80%. (iii) The amount of components having logM < = 3 as measured by GPC is 1.85% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ethylene polymer composition suitable for obtaining an extrusion-molded product such as a pipe having excellent moldability and further excellent long-term performance, and a pipe composed of the same. Background Art

[0002] Ethylene polymers are formed by various molding methods and used for various purposes. For example, it is known that high-pressure low-density polyethylene polymerized by high-pressure free radical polymerization has long chain branches and excellent processability. It is known that linear low-density ethylene-α-olefin copolymers obtained by polymerizing ethylene and α-olefins using Ziegler-Natta catalysts have excellent mechanical strengths such as tensile strength, tear strength, and impact strength, as well as long-term durability represented by environmental stress cracking (ESCR), hot internal pressure creep characteristics of pipes, and slow crack growth characteristics (Slow Crack Growth: SCG). It is known that linear low-density ethylene-α-olefin copolymers obtained by polymerizing ethylene and α-olefins using metallocene catalysts have extremely excellent impact strength and ESCR. It is known that high-density polyethylene can be obtained by polymerizing ethylene alone or copolymerizing ethylene and α-olefins using Ziegler-Natta catalysts, chromium catalysts, metallocene catalysts, etc., and has excellent rigidity and heat resistance.

[0003] In addition, in the case of a single ethylene-based polymer, required physical properties may not be satisfied depending on the application, and therefore many methods of mixing two ethylene-based polymers having different MFR, density, etc. have been proposed (for example, Patent Documents 1 to 3).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-218324

[0007] Patent document 2: EP3293208

[0008] Patent Document 3: Japanese Patent Application No. 2003-531233 Summary of the invention

[0009] Problems to be solved by the invention

[0010] The properties of conventional polyethylene pipes are sufficient in many cases, but in applications requiring higher pressure resistance, such as pipes where internal fluid pressure is applied for a long and / or short period of time, higher pressure resistance is required. Currently, based on the lower confidence limit obtained in accordance with ISO 9080, the MRS is obtained from the classification table of ISO 12162, and the design stress level for determining the type is generally PE100 (MRS 10.0 MPa).

[0011] The object of the present invention is to obtain an ethylene polymer composition suitable for a polyethylene pipe that combines the performance of PE112 (MRS 11.2 MPa or more and less than 12.5 MPa) or above, such as PE125 (MRS 12.5 MPa or more and less than 14.0 MPa) that requires higher creep strength with excellent formability and low sag properties.

[0012] Means for solving problems

[0013] The present invention relates to the following [1] to

[12] .

[0014] [1] An ethylene polymer composition characterized in that it is an ethylene polymer composition comprising 40 to 60% by mass of an ethylene homopolymer (A) and 60 to 40% by mass of a copolymer (B) of ethylene and an α-olefin having 4 or more carbon atoms [ethylene-α-olefin copolymer (B)] (wherein the total amount of (A) + (B) is 100% by mass), wherein the MFR (MFR2) of the ethylene homopolymer (A) measured at a temperature of 190° C. and a load of 2.16 kg is in the range of 100 to 600 g / 10 min,

[0015] The ethylene polymer composition satisfies the following requirements (i) to (iii),

[0016] (i) Density is between 940 and 960 kg / m 3 range,

[0017] (ii) the amount of the component with logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%,

[0018] (iii) The amount of the component having logM ≤ 3 measured by GPC is 1.85% or less.

[0019] [2] The ethylene polymer composition according to item [1], wherein the α-olefin having 4 or more carbon atoms is 1-butene or 1-hexene.

[0020] [3] The ethylene polymer composition according to item [1] or [2], wherein the intrinsic viscosity [η] of the ethylene-α-olefin copolymer (B) is in the range of 7.0 to 14.0 dl / g.

[0021] [4] An ethylene polymer composition as described in any one of items [1] to [3], characterized in that the MFR (MFR5) of the ethylene polymer composition measured at a temperature of 190°C and a load of 5 kg is in the range of 0.03 to 0.3 g / 10 min.

[0022] [5] The ethylene polymer composition according to any one of items [1] to [4], wherein the molecular weight distribution Mw / Mn of the ethylene polymer composition measured by GPC is in the range of 30 to 70.

[0023] [6] The ethylene polymer composition according to any one of items [1] to [5], which is obtained by polymerizing an ethylene homopolymer (A) and an ethylene-α-olefin copolymer (B) using a Ziegler-Natta catalyst.

[0024] [7] A pipe comprising the ethylene polymer composition according to any one of items [1] to [6].

[0025] [8] The tube according to item [7], characterized in that

[0026] The pipe satisfies the following (a) to (d) simultaneously in the hot internal pressure creep test measured in accordance with ISO1167.

[0027] (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours,

[0028] (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours,

[0029] (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more,

[0030] (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

[0031] [9] The tube as described in item [7] or [8] is characterized in that 0.01 to 3 parts by mass of one or more pigments selected from titanium oxide, titanium yellow, phthalocyanine blue, isoindolinone, quinacridone compounds, condensed azo compounds, ultramarine and cobalt blue are added to 100 parts by mass of the ethylene polymer composition.

[0032]

[10] An ethylene polymer composition comprising an ethylene homopolymer and a copolymer of ethylene and an α-olefin having 4 or more carbon atoms, satisfying the following requirements (i) to (vi),

[0033] (i) Density is between 940 and 960 kg / m 3 range,

[0034] (ii) the amount of the component with logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%,

[0035] (iii) the amount of components with logM ≤ 3 as measured by GPC is 1.85% or less,

[0036] (iv) the MFR (MFR5) measured at a temperature of 190°C and a load of 5 kg is in the range of 0.03 to 0.3 g / 10 min,

[0037] (v) the molecular weight distribution (Mw / Mn) measured by GPC is in the range of 30 to 70,

[0038] (vi) The obtained pipe satisfies the following (a) to (d) simultaneously in a hot internal pressure creep test measured in accordance with ISO 1167,

[0039] (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours,

[0040] (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours,

[0041] (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more,

[0042] (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

[0043]

[11] The ethylene polymer composition according to item

[10] , further satisfying the following requirement (vii),

[0044] (vii) The spectrum obtained by GPC measurement showed bimodality, and the content ratio of the low molecular weight component to the high molecular weight component obtained by peak separation was in the range of 40:60 to 60:40.

[0045]

[12] The ethylene polymer composition as described in item

[11] , wherein the low molecular weight side component is composed of an ethylene homopolymer, and the high molecular weight side component is composed of a copolymer of ethylene and an α-olefin having 4 or more carbon atoms.

[0046] Effects of the Invention

[0047] The ethylene polymer composition of the present invention has excellent long-term creep strength and pipe moldability, and the pipe using the ethylene polymer composition of the present invention has excellent long-term creep strength and has performance (PE112) of MRS11.2MPa or more based on ISO 9080 and 12162 classification. Since it has moderate fluidity, it has excellent moldability and low sag property without impairing extrudability during molding.

[0048] The pipe composed of the ethylene polymer composition of the present invention is suitable for water pipelines, gas pipelines and the like. DETAILED DESCRIPTION

[0049] The specific embodiments of the present invention are described in detail below, but the present invention is not limited to the following embodiments and can be implemented with appropriate changes within the scope of the purpose of the present invention. It should be noted that, in this specification, unless otherwise specified, the term "polymer" is used to include homopolymers and copolymers.

[0050] <Ethylene homopolymer (A)>

[0051] The ethylene homopolymer (A) [hereinafter sometimes referred to as "component (A)" or "homopolymer (A)"] as one of the components constituting the ethylene polymer composition of the present invention has an MFR (MFR2) measured at a temperature of 190°C and a load of 2.16 kg in the range of 100 to 600 g / 10 min, preferably in the range of 200 to 500 g / 10 min, and is preferably an ethylene homopolymer polymerized using a Ziegler-Natta catalyst.

[0052] The component (A) of the present invention may also contain a constituent unit derived from at least one monomer (ethylene) derived from biomass. The same type of ethylene constituting the component (A) may be only ethylene derived from biomass, or may contain both ethylene derived from biomass and ethylene derived from fossil fuels. Biomass-derived ethylene refers to ethylene derived from all renewable natural raw materials, such as plant-derived or animal-derived raw materials including fungi, yeast, algae, and bacteria, and their residues, as raw materials, with a 10 -12 The ratio of about 14 The C isotope is carbon, and the biomass carbon concentration (pMC) measured in accordance with ASTM D 6866 is about 100 (pMC). Ethylene derived from biomass can be obtained by a conventionally known method.

[0053] From the viewpoint of reducing environmental burden, it is preferred that component (A) of the present invention contains biomass-derived ethylene.

[0054] The MFR2 of composition (A) of the present invention satisfies above-mentioned scope, thereby the shear viscosity of the ethylene polymer composition comprising composition (A) can not become too high, and the resin pressure of forcing machine reduces, and moldability becomes good.In addition, because low-molecular-weight components can not become too much, so short-term creep strength becomes good.

[0055] The MFR2 of the component (A) of the present invention is measured in accordance with JIS K 7210-1.

[0056] The component (A) of the present invention preferably has an intrinsic viscosity [η] of 0.55 to 0.75 dl / g, more preferably 0.58 to 0.72 dl / g, as measured at 135° C. with a decalin solvent. If the intrinsic viscosity [η] is within the above range, the shear viscosity of the ethylene polymer composition comprising the component (A) will not be too high, the resin pressure of the extruder will be reduced, and the moldability will be good. In addition, since the low molecular weight component will not be too much, the short-term creep strength will be good.

[0057] The preferred density of component (A) of the present invention is 960 kg / m 3 More preferably 965kg / m 3 More preferably, it is between 963 and 973 kg / m 3 The range is preferably between 965 and 971 kg / m 3 If the density of component (A) is within this range, it is easy to make the density of the ethylene polymer composition containing component (A) within the range that satisfies the following requirement (i).

[0058] In addition, the molecular weight distribution (Mw / Mn) of the component (A) of the present invention measured by GPC is preferably in the range of 3.0 to 7.0, more preferably in the range of 4.0 to 6.0. The molecular weight distribution (Mw / Mn) of the component (A) can be obtained by the method of GPC peak separation of the ethylene polymer composition described later. Alternatively, it can be obtained by collecting the component (A) in the manufacturing process of the ethylene polymer composition and measuring it by GPC.

[0059] <Ethylene-α-olefin copolymer (B)>

[0060] The ethylene-α-olefin copolymer (B) [hereinafter sometimes referred to as "component (B)"] as one of the components constituting the ethylene-based polymer composition of the present invention is preferably a copolymer of ethylene and an α-olefin having 4 or more carbon atoms, the intrinsic viscosity [η] of which is preferably in the range of 7.0 to 14 dl / g, more preferably in the range of 8.0 to 12 dl / g as measured with a decalin solvent at 135°C. The α-olefin having 4 or more carbon atoms preferably has 20 or less carbon atoms. The density of component (B) is preferably in the range of 920 to 945 kg / m 3 , more preferably between 925 and 940 kg / m 3 , especially preferably between 930 and 935 kg / m 3In addition, the molecular weight distribution (Mw / Mn) measured by GPC is preferably in the range of 4.0 to 8.0, more preferably in the range of 5.0 to 7.0. The molecular weight distribution (Mw / Mn) of component (B) can usually be obtained by the GPC peak separation method of the ethylene polymer composition described later. Alternatively, in the case where only component (B) can be collected in the manufacturing process of the ethylene polymer composition, it can be obtained by measuring component (B) by GPC.

[0061] When the intrinsic viscosity [η] of the component (B) is within the above range, the creep strength of the ethylene polymer composition containing the component (B) becomes good.

[0062] As the alpha-olefin that forms the carbon number of component (B) of the present invention, it is more than 4, multiple alpha-olefins can be used, specifically can enumerate 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene etc.In these alpha-olefins, preferably 1-butene or 1-hexene, more preferably 1-butene.Aspect manufacturing cost, more preferably 1-butene, but aspect the creep strength of the ethylene polymer composition obtained and molded body, more preferably 1-hexene.

[0063] Component (B) of the present invention may also contain at least one or more biomass-derived ethylene and / or biomass-derived α-olefins. The same type of ethylene and / or α-olefins constituting component (B) may be only biomass-derived ethylene and / or biomass-derived α-olefins, or may contain both biomass-derived ethylene and / or biomass-derived α-olefins and fossil fuel-derived α-olefins and / or fossil fuel-derived ethylene. Biomass-derived ethylene and biomass-derived α-olefins refer to ethylene and α-olefins made from all renewable natural raw materials, such as plant-derived or animal-derived raw materials including fungi, yeast, algae and bacteria, and their residues, with a concentration of 10 -12 The ratio of about 14 The C isotope is carbon, and the biomass carbon concentration (pMC) measured in accordance with ASTM D 6866 is about 100 (pMC). Biomass-derived ethylene and biomass-derived α-olefins can be obtained by conventionally known methods.

[0064] From the viewpoint of reducing environmental burden, it is preferred that component (B) of the present invention contains biomass-derived ethylene and / or α-olefin.

[0065] The component (B) of the present invention preferably has a density of 910 to 960 kg / m 3 , more preferably 922 to 948 kg / m 3 If the density of component (B) is within this range, it is easy to make the density of the ethylene polymer composition containing component (B) within the range that satisfies the following requirement (i).

[0066] The method for producing the component (B) of the present invention is not particularly limited as long as it has the above-mentioned properties, but a polymer polymerized using a multisite catalyst is preferred because it has a broad molecular weight distribution and improves moldability.

[0067] Here, the multisite catalyst refers to a conventionally known catalyst having multiple active sites, such as a Ziegler-Natta catalyst [hereinafter sometimes referred to as a "Ziegler catalyst"], a chromium-based catalyst (Phillips catalyst), a standard catalyst, etc. Among these catalysts, a Ziegler catalyst is preferred.

[0068] 《Ethylene polymer composition》

[0069] The ethylene polymer composition of the present invention {hereinafter, sometimes referred to as "polymer composition"} is characterized in that it is an ethylene polymer composition comprising 40 to 60 mass %, preferably 45 to 58 mass %, more preferably 50 to 56 mass % of the above-mentioned component (A) and 60 to 40 mass %, preferably 55 to 42 mass %, more preferably 50 to 44 mass % of the above-mentioned component (B) [the total amount of (A) + (B) being 100 mass %.], and satisfies the following requirements (i) to (iii).

[0070] <Requirement (i)>

[0071] Density is between 940 and 960 kg / m 3 , preferably between 945 and 958 kg / m 3 , more preferably between 948 and 956 kg / m 3 range.

[0072] When the polymer composition satisfies the above range, the long-term creep strength becomes good.

[0073] 〈Requirement (ii)〉

[0074] The amount of the component having logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%, preferably in the range of 0.38 to 0.75%, and more preferably in the range of 0.40 to 0.70%.

[0075] The polymer composition satisfying the above-mentioned essential factor (ii) can be obtained by making the amount of the contained composition (A) and the composition (B) in the polymer composition be in the above-mentioned scope. In addition, by adjusting the direction that the size of the intrinsic viscosity [η] of the composition (B) increases, the amount of the component of logM ≥ 7 can be controlled to a large direction. And then, in the ethylene polymer composition, there is the larger tendency of the larger amount of the component of logM ≥ 7 of the value of Mz described later.

[0076] By satisfying the above range, the shear viscosity of the polymer composition will not become too high, and the long-term creep strength will become good. If the amount of the component with logM≥7 is too much, the shear viscosity of the polymer composition will become too high, the resin pressure of the extruder will rise, and the moldability may deteriorate. In addition, the appearance when the pipe is made may deteriorate. If the amount of the component with logM≥7 is too little, the long-term creep strength of the polymer composition may decrease.

[0077] <Requirement (iii)>

[0078] The amount of the component having logM ≤ 3 measured by GPC is 1.85% or less, preferably 1.75% or less.

[0079] The polymer composition satisfying the above requirement (iii) can be obtained by making the amounts of component (A) and component (B) contained in the polymer composition within the above range. The amount of the component with logM≤3 is affected by the type and concentration of the catalyst and electron donor used during the production, and other polymerization conditions, but generally, by adjusting the intrinsic viscosity [η] of component (A) in a large direction, the amount of the component with logM≤3 can be adjusted in a smaller direction. In addition, in addition to the intrinsic viscosity [η] of component (A), the content of component (A) also affects the amount of the component with logM≤3. Generally, the more the content of component (A) is reduced, the smaller the amount of the component with logM≤3 becomes. Furthermore, with respect to the hexane used in the polymerization solvent, by increasing the proportion of the hexane solvent (recycled hexane) obtained by centrifuging the polymer slurry containing the mother liquor after the reaction in the second polymerization tank and returning it to the polymerization tank again, the low molecular weight components contained in the recycled hexane are incorporated into the polymer in large quantities, and the amount of the component with logM≤3 is increased. That is, by reducing the ratio of the recycled hexane returned to the polymerization layer, the amount of the component with logM≤3 can be adjusted to decrease.

[0080] The lower limit of the amount of the component having logM ≤ 3 in the polymer composition is not particularly limited, but is usually 0.50% or more or 1.00% or more.

[0081] By suppressing the amount of the component with logM≤3 in the polymer composition to 1.85% or less, the long-term creep strength becomes good.

[0082] Regarding the ethylene polymer composition of the present invention, in addition to the above-mentioned requirements (i) to (iii), the molecular weight distribution (Mw / Mn) measured by GPC is preferably in the range of 30 to 70, more preferably in the range of 40 to 65, further preferably in the range of 45 to 65, and especially preferably in the range of 50 to 65.

[0083] If the Mw / Mn of the polymer composition of the present invention is too low, the shear viscosity of the polymer composition becomes too high, the resin pressure of the extruder increases, and the moldability may deteriorate. In addition, if the Mw / Mn is too high, poor mixing of component (A) and component (B) may occur, and the appearance during pipe molding may deteriorate.

[0084] The spectrum obtained by GPC measurement of the polymer composition of the present invention generally shows a bimodal molecular weight distribution.

[0085] In addition to the above requirements (i) to (iii), the ethylene polymer composition of the present invention preferably has a Z average molecular weight (Mz) measured by GPC of 2.0×10 6 More preferably, 3.0×10 6 More preferably, 4.0×10 6 The upper limit is usually 5.5×10 6 Below, or 5.0×10 6 the following.

[0086] In addition, in the ethylene polymer composition of the present invention, the ratio of Mw / Mn of component (A) to Mw / Mn of component (B), (Mw / Mn(B)) / (Mw / Mn(A)), is preferably greater than 0.9, more preferably greater than 1.0, and further preferably greater than 1.1.

[0087] The polymer composition of the present invention preferably has an MFR (MFR5) measured at a temperature of 190° C. and a load of 5 kg in the range of 0.03 to 0.3 g / 10 min, more preferably in the range of 0.05 to 0.25 g / 10 min.

[0088] When the MFR5 of the copolymer composition satisfies the above range, the creep strength becomes good while the moldability and low sag property are maintained.

[0089] In addition, the MFR (hereinafter referred to as MFR) of the ethylene polymer composition of the present invention at 190°C and a load of 21.6 kg is 21.6 ) and MFR5 ratio (MFR 21.6 / MFR5) is 40 or more, preferably 50 or more. 21.6 Ratio to MFR5 (MFR 21.6 / MFR5) is usually less than 100. By using MFR 21.6 An ethylene polymer composition having / MFR5 within the above range can provide a polyethylene pipe having excellent moldability and excellent fracture stress resistance and thermal internal pressure creep resistance.

[0090] The MFR (MFR5 and MFR 21.6) is measured in accordance with JIS K 7210-1.

[0091] 《Ethylene polymer composition 2》

[0092] The ethylene polymer composition of the present invention can also be defined as follows (hereinafter referred to as "ethylene polymer composition 2").

[0093] The ethylene polymer composition 2 of the present invention is an ethylene polymer composition comprising an ethylene homopolymer and a copolymer of ethylene and an α-olefin having 4 or more carbon atoms and satisfying the following requirements (i) to (vi).

[0094] (i) Density is between 940 and 960 kg / m 3 range.

[0095] (ii) The amount of the component having logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%.

[0096] (iii) The amount of the component having logM ≤ 3 measured by GPC is 1.85% or less.

[0097] (iv) MFR (MFR5) measured at a temperature of 190°C and a load of 5 kg is in the range of 0.03 to 0.3 g / 10 min.

[0098] (v) The molecular weight distribution (Mw / Mn) measured by GPC is in the range of 30 to 70.

[0099] (vi) The obtained pipe satisfies the following (a) to (d) simultaneously in a hot internal pressure creep test measured in accordance with ISO1167.

[0100] (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours,

[0101] (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours,

[0102] (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more,

[0103] (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

[0104] The above requirements (i) to (v) are as described in detail in this specification, and the requirement (vi) is as described later in the section on pipes.

[0105] The ethylene polymer composition 2 preferably further satisfies the following requirement (vii).

[0106] (vii) The spectrum obtained by GPC measurement shows bimodality, and the content ratio of the low molecular weight component and the high molecular weight component obtained by peak separation is in the range of 40:60 to 60:40, more preferably in the range of 50:50 to 60:40, and even more preferably in the range of 55:45 to 60:40.

[0107] Regarding the peak separation of the GPC spectrogram, it is possible to obtain the peak separation by curve fitting the bimodal peaks appearing in the molecular weight distribution curve with two normal distribution curves. In addition, it is also possible to obtain the peak separation by performing overall GPC determination, using commercially available data analysis software, etc., to obtain the multimodal molecular weight distribution curve by calculating its component ratio. For example, based on a program made using Visual Basic using Microsoft Excel (registered trademark), the two separated peak curves are set to lognormal distribution, and the molecular weight distribution curve is separated into two peak curves with different molecular weights by convergence calculation. The curve obtained by resynthesizing the two separated peak curves is compared with the GPC spectrogram, and the calculation is performed while changing the initial value in a manner that makes the two almost identical. The calculation is performed as follows: Log (molecular weight) [LogM] is divided at 0.02 intervals, and the intensity is standardized in a manner that the area of ​​the measured molecular weight curve and the area of ​​the curve obtained by resynthesizing the two separated peak curves become 1.

[0108] The low molecular weight component corresponds to the component (A) constituting the above-mentioned ethylene polymer composition, and the high molecular weight component corresponds to the component (B) constituting the above-mentioned ethylene polymer composition.

[0109] In order to achieve the physical properties shown in the above-mentioned requirement (vi), it is desirable that the low molecular weight side component is composed of an ethylene homopolymer. According to the production method described below, an ethylene homopolymer (A) can be produced. In addition, at this time, the high molecular weight side component is composed of a copolymer of ethylene and an α-olefin having more than 4 carbon atoms.

[0110] In addition, the requirements that the ethylene-based polymer composition 2 preferably satisfies are the same as those already described for the ethylene-based polymer composition.

[0111] Pigments and Additives

[0112] In the ethylene polymer composition of the present invention, it is preferred to add 0.01 to 3 parts by mass of one or more pigments selected from titanium oxide, titanium yellow, phthalocyanine blue, isoindolinone, quinacridone compounds, condensed azo compounds, ultramarine and cobalt blue, with respect to 100 parts by mass of the polymer composition (total amount of (A) + (B)), and it is further preferred to add 0.05 to 2 parts by mass. By adding the pigment, a tube suitable for a water pipe or a gas pipe can be obtained. The color of the tube is, for example, blue, yellow, orange, white, red, green, purple, etc.

[0113] In addition, in the ethylene polymer composition of the present invention, preferably 0.01 to 3 parts by mass, preferably 0.5 to 2.5 parts by mass, and more preferably 2.0 to 2.5 parts by mass of carbon black is added to 100 parts by mass of the polymer composition (the total amount of (A) + (B)). By adding carbon black, a pipe suitable for a water pipe or a gas pipe having excellent weather resistance can be obtained. In this case, the color of the pipe is black, gray, etc.

[0114] In addition, in ethylene polymer composition of the present invention, can be on the basis that polymer composition is added other resins, be used for various molded body purposes described later.As other resins, ethylene resins, polyolefin rubbers such as high density polyethylene, low density polyethylene, very low density polyethylene, ultra low density polyethylene can be exemplified, as addition, for example, be below 10 mass parts with respect to polymer composition (total amount of (A)+(B)) 100 mass parts.

[0115] The ethylene polymer composition of the present invention can be formulated with additives commonly used in olefin polymers, such as weather stabilizers, heat stabilizers, antistatic agents, anti-slip agents, anti-blocking agents, anti-fogging agents, lubricants, dyes, nucleating agents, plasticizers, antioxidants, hydrochloric acid absorbers, antioxidants, etc., as needed without impairing the purpose of the present invention.

[0116] 《Method for producing ethylene polymer composition》

[0117] Polymer composition of the present invention is preferably manufactured by slurry polymerization of the above-mentioned ethylene homopolymer (A) and the above-mentioned ethylene-α-olefin copolymer (B) that will constitute the ethylene polymer composition by using MgCl2 system's Ziegler-Natta catalyst. Component (A), component (B) can be separately polymerized respectively, and also can carry out multistage polymerization. Under the situation of separate polymerization separately, by utilizing known method in the past each component (A, B) is mixed or melt-mixed, thereby obtains the ethylene polymer composition. For example, by using forcing machine, Brabender internal mixer (Brabender Plastograph), Banbury mixer, kneader etc. each component (A, B) is melted, mixed, thereby obtains the ethylene polymer composition. Under the situation of multistage polymerization, the dispersibility of each component (A, B) becomes good, and the outward appearance of the pipe molded by the ethylene polymer composition of the present invention becomes good.

[0118] 《Molding body, tube》

[0119] Ethylene polymer composition of the present invention is obtained various molded bodies by molding, thereby can be used for known various purposes of ethylene resin.Wherein, ethylene polymer composition of the present invention is suitable for pipe purposes.The pipe moldability of ethylene polymer composition of the present invention is excellent, and by molding, pipe and multilayer pipe with excellent long-term durability can be obtained.Here, at least one layer of this multilayer pipe is formed by the layer consisting of the above-mentioned copolymer composition of the present invention.In this multilayer pipe molded body, the layer consisting of the copolymer composition can only be formed on one side, can also be formed on both sides, and can also be matched with the pigment of above-mentioned "other matching components" on one side formed in the two sides.The base material constituting this multilayer pipe can be constituted by the copolymer composition, or can also be constituted by the material beyond the copolymer composition.

[0120] When the tube is multi-layered, other resins are not particularly limited, and examples thereof include crystalline resins, rubbers, adhesive resins, barrier resins, and the like. Specifically, examples thereof include high-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, ultra-low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid copolymers, ethylene-methacrylate copolymers, ethylene-vinyl alcohol copolymers, ethylene-vinyl acetate copolymer saponification products, ethylene-styrene copolymers, ethylene-vinyl cyclohexane copolymers, ethylene-norbornene copolymers, polyolefin rubbers, styrene-butadiene rubbers, styrene-butadiene-styrene block copolymers, isoprene rubbers, styrene-isoprene rubbers, isobutylene rubbers, and acid-modified products and hydrogenated products of these resins.

[0121] The pipe of the present invention is obtained by molding the copolymer composition of the present invention using a known pipe molding method, for example, by using an extruder of a pipe manufacturing device, dissolving the copolymer composition at a temperature of 150° C. to 220° C., preferably 160° C. to 210° C., extruding it from a die into a cylindrical shape, and cooling it with water.

[0122] The shape of the pipe of the present invention can be appropriately determined according to the purpose of the pipe. For example, it includes a polyethylene pipe molded into an outer diameter and a wall thickness recorded in ISO4427, ISO4437, JIS K6761, JIS K6762 or JIS K6774. In addition, these molded bodies include: a molded body (laminated body, etc.) comprising a part consisting of an ethylene polymer composition and a part consisting of other resins.

[0123] The pipe of the present invention is characterized by satisfying the following (a) to (d) simultaneously in a hot internal pressure creep test measured in accordance with ISO1167.

[0124] (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours,

[0125] (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours,

[0126] (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more,

[0127] (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

[0128] Example

[0129] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.

[0130] In addition, the measuring method of the characteristics and the measuring method of the physical property of each component used in the Example are as follows.

[0131] (1) 2.16 kg load melt flow rate (MFR2, g / 10 min)

[0132] The measurement was performed in accordance with JIS K 7210-1 at 190° C. and under a load of 2.16 kg.

[0133] (2) Melt flow rate at 5 kg load (MFR5, g / 10 min)

[0134] The measurement was performed at 190° C. and under a load of 5 kg in accordance with JIS K 7210-1.

[0135] (3) Melt flow rate (MFR) at 21.6 kg load 21.6 , g / 10 minutes)

[0136] The measurement was performed in accordance with JIS K 7210-1 at 190° C. and under a load of 21.6 kg.

[0137] (4) Density (kg / m 3 )

[0138] The density was measured by a density gradient tube method in accordance with JIS K 7112 by heat-treating the line obtained in the MFR measurement at 100° C. for 1 hour and then leaving it at room temperature for 1 hour.

[0139] Regarding the density (D B ), using the following formula (Eq-1), the mass fraction BR of the ethylene homopolymer (A) is A , density D A and the density D of the ethylene polymer composition C Come and ask for it.

[0140] BR B / D B =(1 / D C )-(BR A / D A )------------(Eq-1)

[0141] (5) Intrinsic viscosity ([η], dl / g)

[0142] Regarding the intrinsic viscosity, about 20 mg of the sample was dissolved in 15 ml of decalin, and the specific viscosity ηsp was measured in an oil bath at 135°C. After diluting the decalin solution by adding 5 ml of decalin solvent, the specific viscosity ηsp was measured in the same manner. The dilution operation was repeated twice, and the value of ηsp / C when the concentration (C) was extrapolated to 0 was calculated as shown in the following formula (Eq-2), which was taken as the intrinsic viscosity [η] (unit: dl / g).

[0143] [η]=lim(ηsp / C)(C→0)------------(Eq-2)

[0144] In addition, regarding the intrinsic viscosity ([η]) of the ethylene-α-olefin copolymer (B) in the multistage polymerization, B ), using the following formula (Eq-3), the mass fraction BR of the ethylene homopolymer A 、Intrinsic viscosity [η] A and the intrinsic viscosity [η] of the ethylene polymer compositionC Come and ask for it.

[0145] [η] B =([η] C -[η] A ×BR A ) / (1-BR A )------------(Eq-3)

[0146] (6) logM≥7 component weight, logM≤3 component weight

[0147] The amount of the component with logM≥7 was measured as follows using a gel permeation chromatograph HLC-8321GPC / HT manufactured by Tosoh Corporation.

[0148] Analysis software: Chromatography Data System Empower3 (Waters, registered trademark), chromatographic columns: TSKgelGMH6-HT×2+TSKgel GMH6-HTL×2 (inner diameter 7.5 mm×length 30 cm, manufactured by Tosoh Corporation), mobile phase: o-dichlorobenzene (Wako Pure Chemical Industries, Ltd. special grade reagent), detector: differential refractometer (built-in device), column temperature: 140°C, flow rate: 1.0 mL / min, injection volume: 400 μL, sampling time interval: 0.5 sec, sample concentration: 0.1% (w / v), molecular weight calibration: monodisperse polystyrene (manufactured by Tosoh Corporation); #3std set.

[0149] The molecular weight distribution curve was prepared by conversion using the molecular weight of standard polyethylene according to the universal calibration procedure described in Z. Crubisic, P. Rempp, H. Benoit, J. Polym. Sci., B5, 753 (1967).

[0150] About the component amount of logM ≥ 7, the molecular weight distribution curve (G1) of the obtained ethylene polymer composition is calculated by the following method. It should be noted that in this manual, when claiming "molecular weight distribution curve", as long as there is no special restriction, it refers to the differential molecular weight distribution curve, in addition, about the molecular weight distribution curve, when claiming "area", it refers to the area in the zone formed between the molecular weight distribution curve and the baseline.

[0151] In each numerical data of (G1), Log (molecular weight, hereinafter referred to as M) was divided into intervals of 0.02, and the intensity [dwt / d(logM)] was normalized so that the area became 1 for each (G1).

[0152] Then, the sum of the normalized dwt / dlogM when logM≥7 was calculated as the amount of the component with logM≥7. Similarly, the sum of the normalized dwt / dlogM when logM≤3 was calculated as the amount of the component with logM≤3.

[0153] (7) Molecular weight distribution (Mw / Mn), average molecular weight (Mw, Mn, Mz)

[0154] Mw / Mn is calculated by the method of (6) above from the weight average molecular weight (Mw), number average molecular weight (Mn), and z average molecular weight (Mz) calculated as standard polyethylene molecular weights.

[0155] (7-2) Peak separation of molecular weight distribution

[0156] The bimodal peaks appearing in the molecular weight distribution curve were fitted with two normal distribution curves to separate the peaks, and the content ratio of each component and the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of each component were determined.

[0157] (8) Thermal internal pressure creep test failure time

[0158] <Tube Forming Method>

[0159] The ethylene polymer composition (C) was extruded using a 65 mmφ, L / D=25 pipe forming machine manufactured by Ikegai Iron Works Co., Ltd. at a set temperature of 200°C and an extrusion rate of 22 kg / hr to obtain a polyethylene pipe with SDR=11 and 60 mmφ.

[0160] <Internal pressure creep failure time>

[0161] The tube length is 50 cm, the temperature is 20°C or 80°C, the circumferential stress at 20°C is in the range of 11 to 15 MPa, and the circumferential stress at 80°C is in the range of 5 to 7 MPa, and the measurement is carried out in accordance with ISO 1167.

[0162] (9) 80℃ tensile fatigue strength (FNFT failure stress: MPa)

[0163] A prism of 6 mm in length x 6 mm in width x 60 mm in length was cut out from the obtained polyethylene tube to prepare an evaluation sample. The tensile fatigue strength (test piece shape) was measured in accordance with JIS K 6774. The test conditions of full circumference notch type and notch depth of 1 mm are summarized as follows.

[0164] The fatigue strength is determined by measuring the number of times the sample is broken at the time of failure in the range of the test piece shape (6mm×6mm×60mm prism with notch), test waveform and test frequency (rectangular wave, 0.5Hz), test temperature 80℃, and actual stress 10-18MPa. In addition, the fatigue strength is determined by measuring at least 3 points with different actual stresses, measuring at the range of the number of fractures in the third digit or more or the actual stress in the range of 3MPa or more, and making an approximate formula using the least square method of power approximation to obtain the actual stress corresponding to the number of fractures of 10,000 and 100,000.

[0165] [Example 1]

[0166] <Production of ethylene homopolymer (A-1)>

[0167] As the catalyst, a MgCl2-based Ziegler-Natta catalyst was used.

[0168] Internal volume 0.34m 3 70.7 L / hr of n-hexane, 1.9 mmol-Ti / hr of catalyst, and 11 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer (A) was polymerized under the conditions of polymerization temperature of 85°C, reaction pressure of 0.65 MPaG, and average residence time of 2.0 hr. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.4 mol / mol)

[0169] The content continuously withdrawn from the first polymerization tank was subjected to a flash drum maintained at an internal pressure of 0.03 MPa and 30° C. to substantially remove unreacted ethylene and hydrogen.

[0170] The physical properties of the homopolymer (A-1) from which unreacted ethylene and hydrogen were substantially removed were measured by the methods described above.

[0171] <Production of Copolymer (B-1) and Copolymer Composition (C-1)>

[0172] Afterwards, the contents are continuously supplied to the inner volume of 0.2m 3In the second polymerization tank, ethylene-1-butene copolymer (B-1) was polymerized under the conditions of n-hexane 57L / hr, polymerization temperature 72°C, reaction pressure 0.30MPaG, and average residence time 1.0hr. During the polymerization, ethylene, 1-butene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.031kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene = 0.016mol / mol. In the second polymerization tank, the contents of the polymerization tank were also continuously drawn out to keep the liquid level in the polymerization tank fixed, and the n-hexane and unreacted monomers in the contents were removed by a solvent separation device, and dried to obtain an ethylene-based polymer composition (C-1) containing a homopolymer (A-1) and an ethylene-1-butene copolymer (B-1). The yield of the obtained copolymer composition (C-1) was 16kg / hr.

[0173] The amount and physical properties of the copolymer (B-1) contained in the composition (C-1) and the physical properties of the composition (C-1) were measured by the methods described above.

[0174] Next, 0.15 parts by mass of calcium stearate as a hydrochloric acid absorber, 0.2 parts by mass of Irganox 1010 manufactured by BASF as an antioxidant, 0.1 parts by mass of Irgafos 168 manufactured by BASF, and 0.1 parts by mass of Tinuvin 622LD manufactured by BASF were added to 100 parts by mass of the copolymer composition, and the mixture was melt-kneaded using a GM40-28 extruder manufactured by GM Sansei Co., Ltd. at a set temperature of 200° C. and a screw speed of 80 rpm, and then extruded into a strand shape and cut to obtain pellets.

[0175] The physical properties of the pellets of the obtained ethylene polymer composition are shown in Table 1. In addition, a tube was molded by the above method, and the performance thereof was evaluated. The results are shown in Table 2.

[0176] [Example 2]

[0177] Internal volume 0.34m 3 71.8 L / hr of n-hexane, 1.9 mmol-Ti / hr of the same catalyst as in Example 1, and 14 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer (A-2) was polymerized under the same polymerization temperature, reaction pressure, and average residence time of 1.9 hr as in Example 1. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.3 mol / mol)

[0178] The (A-2) extracted from the first polymerization tank was continuously supplied to a 0.2 m3 In the second polymerization tank, ethylene-1-butene copolymer (B-2) was polymerized under the same conditions as in Example 1. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.031 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene = 0.017 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 17 kg / hr.

[0179] In addition, the amount and physical properties of (B-2) contained in the composition (C-2), the physical properties of the composition (C-2), and the tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0180] [Example 3]

[0181] Internal volume 0.34m 3 70.4 L / hr of n-hexane, 1.9 mmol-Ti / hr of the same catalyst as in Example 1, and 11 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer (A-3) was polymerized under the same polymerization temperature, reaction pressure, and average residence time of 1.9 hr as in Example 1. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.2 mol / mol)

[0182] The (A-3) extracted from the first polymerization tank was continuously supplied to a 0.2 m 3 In the second polymerization tank, ethylene-1-butene copolymer (B-3) was polymerized under the same conditions as in Example 1. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.018 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene = 0.007 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 17 kg / hr.

[0183] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0184] [Comparative Example 1]

[0185] Internal volume 0.34m 370.3 L / hr of n-hexane, 1.9 mmol-Ti / hr of the same catalyst as in Example 1, and 11 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer was polymerized under the same polymerization temperature, reaction pressure, and average residence time of 1.9 hr as in Example 1. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.2 mol / mol)

[0186] The contents extracted from the first polymerization tank were continuously supplied to a 0.2 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Example 1. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.043 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.007 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 20 kg / hr.

[0187] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0188] [Comparative Example 2]

[0189] Internal volume 0.34m 3 73.6 L / hr of n-hexane, 1.9 mmol-Ti / hr of the same catalyst as in Example 1, and 15 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, while ethylene homopolymer was polymerized under the same conditions as in Example 1. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.5 mol / mol)

[0190] The contents extracted from the first polymerization tank were continuously supplied to a 0.2 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Example 1. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.050 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene = 0.025 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 17 kg / hr.

[0191] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0192] [Comparative Example 3]

[0193] Internal volume 0.34m 3 68L / hr of n-hexane, 3.8mmol-Ti / hr of the same catalyst as in Example 1, and 50mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer was polymerized under the conditions of polymerization temperature of 85°C, reaction pressure of 0.6MPaG, and average residence time of 2.0hr. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.1mol / mol)

[0194] The contents extracted from the first polymerization tank were continuously supplied to a 0.2 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the conditions of polymerization temperature 72°C, reaction pressure 0.3MPaG, and average residence time 1.0hr. During the polymerization, ethylene, 1-butene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.077kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.020mol / mol. For the obtained contents, the solvent and unreacted monomers were separated in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 19kg / hr.

[0195] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0196] [Comparative Example 4]

[0197] Internal volume 0.34m 3 68 L / hr of n-hexane, 3.2 mmol-Ti / hr of the same catalyst as in Example 1, and 50 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, and ethylene homopolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 4.8 mol / mol)

[0198] The contents taken out from the first polymerization tank were continuously supplied to a 0.2 m 3In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same polymerization temperature, reaction pressure and average residence time of 1.1 hr as in Comparative Example 3. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.077 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.011 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 17 kg / hr.

[0199] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0200] [Comparative Example 5]

[0201] Internal volume 0.34m 3 68 L / hr of n-hexane, 3.1 mmol-Ti / hr of the same catalyst as in Example 1, and 50 mmol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, and ethylene homopolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.4 mol / mol)

[0202] The contents extracted from the first polymerization tank were continuously supplied to a 0.2 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.062 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.017 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 19 kg / hr.

[0203] In addition, physical property measurement, tube molding and performance evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0204] [Example 4]

[0205] Internal volume 60m 314850 L / hr of n-hexane, 1.1 mol-Ti / hr of the same catalyst as in Example 1, and 7.4 mol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, and ethylene homopolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.9 mol / mol)

[0206] The contents extracted from the first polymerization tank were continuously supplied to a 60 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.018 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.021 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 11000 kg / hr.

[0207] [Example 5]

[0208] Internal volume 60m 3 14850 L / hr of n-hexane, 1.1 mol-Ti / hr of the same catalyst as in Example 1, and 7.4 mol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, and ethylene homopolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.9 mol / mol)

[0209] The contents extracted from the first polymerization tank were continuously supplied to a 60 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.010 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.016 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 11000 kg / hr.

[0210] [Reference Example 1]

[0211] Internal volume 60m 320200L / hr of n-hexane, 1.6mol-Ti / hr of the same catalyst as in Example 1, and 10mol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant. At the same time, ethylene homopolymer was polymerized under the conditions of polymerization temperature of 87°C, reaction pressure of 0.6MPaG, and average residence time of 2.0hr. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 6.4mol / mol)

[0212] The contents extracted from the first polymerization tank were continuously supplied to a 60 m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the conditions of polymerization temperature 84°C, reaction pressure 0.3MPaG, and average residence time 1.0hr. During the polymerization, ethylene, 1-butene, hydrogen, and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.02kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.047mol / mol. For the obtained contents, the solvent and unreacted monomers were separated in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 16000kg / hr.

[0213] [Reference Example 2]

[0214] Internal volume 60m 3 19600 L / hr of n-hexane, 1.3 mol-Ti / hr of the same catalyst as in Example 1, and 9.8 mol-Al / hr of triethylaluminum were continuously supplied to the first polymerization tank, and the contents of the polymerization tank were continuously withdrawn to keep the liquid level in the polymerization tank constant, and ethylene homopolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, hydrogen, and nitrogen were continuously supplied to maintain a constant gas composition. (Gas composition (molar ratio): hydrogen / ethylene = 5.2 mol / mol)

[0215] The contents extracted from the first polymerization tank were continuously supplied to the inner volume 60m 3 In the second polymerization tank, ethylene-1-butene copolymer was polymerized under the same conditions as in Comparative Example 3. During the polymerization, ethylene, 1-butene, hydrogen and nitrogen were continuously supplied to maintain a fixed gas composition. The supply ratio of 1-butene to ethylene was 0.069 kg / kg, and the gas composition (molar ratio) of hydrogen to ethylene was: hydrogen / ethylene=0.057 mol / mol. The obtained contents were separated from the solvent and unreacted monomers in the same manner as in Example 1, and dried to obtain an ethylene-based polymer composition. The output was 13200 kg / hr.

[0216] [Comparison between Examples and Comparative Examples]

[0217] It is found that Examples 1 to 3 are significantly superior in internal pressure creep rupture time at 80°C and σ=5.7 MPa compared to Comparative Examples 3 to 5 in which the amount of the component with logM ≥ 7 does not satisfy requirement (ii).

[0218] Compared with Comparative Examples 1 and 2, in which the amount of components with logM ≥ 7 satisfies requirement (ii) but the amount of components with logM ≤ 3 does not satisfy requirement (iii), Examples 1 to 3 have significantly superior internal pressure creep rupture times at 20°C, σ = 12.7 MPa, 80°C, σ = 6.3 MPa, and 80°C, σ = 6.1 MPa.

[0219] That is, it can be said that the pipes obtained in Examples 1 to 3 are excellent in internal pressure creep rupture time under a wide range of temperature and pressure conditions.

[0220] [Table 1]

[0221]

[0222] [Table 2]

[0223]

[0224] Industrial Applicability

[0225] The ethylene polymer composition of the present invention having excellent moldability and mechanical strength can be suitably used for pipe applications such as water pipes and gas pipes.

Claims

1. An ethylene polymer composition, characterized in that An ethylene polymer composition comprising 40 to 60% by weight of an ethylene homopolymer (A) and 60 to 40% by weight of a copolymer (B) of ethylene and an α-olefin having 4 or more carbon atoms, wherein the MFR (MFR2) of the ethylene homopolymer (A) measured at a temperature of 190° C. and a load of 2.16 kg is in the range of 100 to 600 g / 10 min, wherein the total amount of (A) + (B) is 100% by weight, The ethylene polymer composition satisfies the following requirements (i) to (iii), (i) Density is between 940 and 960 kg / m 3 range, (ii) the amount of the component with logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%, (iii) The amount of the component having logM ≤ 3 measured by GPC is 1.85% or less.

2. Ethylene polymer composition as claimed in claim 1, characterized in that, The α-olefin having 4 or more carbon atoms is 1-butene or 1-hexene.

3. Ethylene polymer composition as claimed in claim 1, is characterized in that, The intrinsic viscosity η of the ethylene-α-olefin copolymer (B) is in the range of 7.0 to 14.0 dl / g.

4. Ethylene polymer composition as claimed in claim 1, characterized in that, The MFR5 of the ethylene polymer composition measured at a temperature of 190° C. and a load of 5 kg is in the range of 0.03 to 0.3 g / 10 min.

5. Ethylene polymer composition as claimed in claim 1, wherein, The molecular weight distribution Mw / Mn of the ethylene polymer composition measured by GPC is in the range of 30-70.

6. The ethylene polymer composition according to claim 1, which is obtained by polymerizing an ethylene homopolymer (A) and an ethylene-α-olefin copolymer (B) using a Ziegler-Natta catalyst. 7 . A pipe comprising the ethylene polymer composition according to claim 1 .

8. The tube according to claim 7, characterized in that The pipe satisfies the following (a) to (d) simultaneously in the hot internal pressure creep test measured in accordance with ISO1167. (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours, (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours, (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more, (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

9. The tube according to claim 7, characterized in that The present invention comprises adding 0.01 to 3 parts by mass of one or more pigments selected from carbon black, titanium oxide, titanium yellow, phthalocyanine blue, isoindolinone, quinacridone compounds, condensed azo compounds, ultramarine blue and cobalt blue to 100 parts by mass of the ethylene polymer composition.

10. An ethylene polymer composition, which is composed of an ethylene homopolymer and a copolymer of ethylene and an α-olefin having 4 or more carbon atoms, and satisfies the following requirements (i) to (vi), (i) Density is between 940 and 960 kg / m 3 range, (ii) the amount of the component with logM ≥ 7 measured by GPC is in the range of 0.35 to 0.80%, (iii) the amount of components with logM ≤ 3 as measured by GPC is 1.85% or less, (iv) MFR5 measured at a temperature of 190°C and a load of 5 kg is in the range of 0.03 to 0.3 g / 10 min, (v) the molecular weight distribution Mw / Mn measured by GPC is in the range of 30 to 70, (vi) The obtained pipe satisfies the following (a) to (d) simultaneously in a hot internal pressure creep test measured in accordance with ISO 1167, (a) The failure time at the test temperature of 20°C and the test circumferential stress of 12.7 MPa is more than 500 hours, (b) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.3 MPa is more than 100 hours, (c) The time to failure at a test temperature of 80°C and a test circumferential stress of 6.1 MPa is 1,000 hours or more, (d) The time to failure at a test temperature of 80°C and a test circumferential stress of 5.7 MPa is 3,000 hours or more.

11. The ethylene polymer composition of claim 10, further satisfying the following requirement (vii), (vii) The spectrum obtained by GPC measurement showed bimodality, and the content ratio of the low molecular weight component to the high molecular weight component obtained by peak separation was in the range of 40:60 to 60:

40.

12. Ethylene polymer composition as claimed in claim 11, wherein, The low molecular weight component is composed of an ethylene homopolymer, and the high molecular weight component is composed of a copolymer of ethylene and an α-olefin having 4 or more carbon atoms.