High refractive index composition for coating of optical substrate and use thereof
By using a high-refractive black coating composed of curable polymer and metal oxide nanoparticles on a high-refractive index optical substrate, the problem of reflection and scattering of traditional coatings on a high-refractive index substrate is solved, achieving efficient edges Blackening and stray light control.
Patent Information
- Application Number
- CN202380018577.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-24
- Filing Date
- 2023-01-23
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional edge blackening coatings do not perform well on high-refractive index optical substrates, making it difficult to effectively reduce reflection at the optical substrate-coating interface, and light reenters the substrate due to light absorption and scattering, affecting system performance.
A high-refractive index black coating consisting of curable polymers, metal oxide nanoparticles and black pigments is used to form a film by curing to ensure that the high refractive index of the coating matches the optical substrate, reduce reflection and control optical density.
Efficient edge blackening and stray light control on high-refractive index optical substrates are achieved, which significantly reduces reflection at the optical substrate-coating interface and optimizes viscosity by adjusting optical density and particle size, improving the application adaptation of coatings. sex.
Smart Images

Figure BDA0004960547500000011 
Figure BDA0004960547500000181 
Figure BDA0004960547500000202
Abstract
Description
Technical Field
[0001] The present invention relates to coatings of optical substrates using curable compositions containing fillers. More particularly, the present invention relates to black coatings on optical substrates, compositions for preparing such coatings, and the use of said compositions in edge blackening and stray light control. Background Art
[0002] Edge blackening coatings are applied to the edge of an optical substrate, or at specific limited locations of an optical substrate, specifically on the substrate where light propagates within the substrate. Typically, the coating is applied to optical components such as lenses, prisms, beam splitters, waveguides, or diffractive optical elements to minimize unwanted reflections of light propagating within the optical substrate from the substrate-air interface. In addition, edge blackening minimizes light that enters the optical substrate through the coated area. The edge area typically includes an unpolished rough surface. Light reflected from the edge typically results in stray light, which is a common limiting factor for optical system performance.
[0003] By applying an edge black coating, the reflection of light reaching the substrate-air interface can be minimized, and for optimal performance, the coating needs to be Figure 1 The three effects depicted in FIG. 1 are minimized. These effects are: 1) reflection at the substrate-coating interface, 2) light entering the substrate from within the optical coating due to reflection at the coating-air interface or light entering the coating from the outside, and 3) re-entry into the optical substrate due to scattering within the optical coating.
[0004] In order to Figure 1 ), the material used for the coating should have a refractive index that matches that of the substrate, and more specifically, have a real part of the complex refractive index that matches that of the substrate. However, conventional edge blackening coatings do not have a high refractive index, so they do not perform well on high refractive index (RI) substrates. The k value, i.e., the complex part of the RI, is always non-zero in black materials (i.e., absorbing materials), and it contributes partially to the reflectivity. Optical substrates are typically highly transparent to light of the desired wavelength, which indicates that the k value is close to zero. As an example, at normal incidence, the reflectivity R at the interface of a transparent substrate and an absorbing coating is expressed by the following equation:
[0005]
[0006] Among them, n s and n c are the real parts of the complex refractive index of the substrate and coating, respectively, k c is the complex part of the refractive index of the coating. Even if the real part of the RI is matched and the k value of the coating is high (>0.05), the reflectivity due to the k value mismatch can make a meaningful contribution to the reflected component 1.
[0007] Once light has entered the optical coating, the light absorbing properties of the material (i.e., the black color of the material) prevents it from re-entering the optical substrate (component 2, Figure 1 ). The absorbance or optical density of the material at the desired wavelength of light (usually that of visible light) should be high enough so that only minimal intensity of light re-enters from the black coating. Another re-entry mechanism is scattering in the edge black coating (component 3, Figure 1 ), resulting in diffuse reflection of the incident light.
[0008] The refractive index is usually increased by using high refractive index fillers. When the refractive index is increased above 1.75 at 589 nm, especially above 1.80, the required weight content of filler particles is significant (unless the formulation is carefully balanced), otherwise the use of the material is limited due to high viscosity and poor coating properties. Summary of the invention
[0009] The present invention is based on the concept of providing a black coating including a film formed by curing a composition of a curable polymer and a curable monomer mixed with high refractive index nanoparticles and a black pigment.
[0010] In one embodiment, the black coating comprises a film formed from a photocurable composition mixed with metal oxide nanoparticles and a black pigment, and the cured solid film has a weight percentage of metal oxide nanoparticles greater than 45%, specifically greater than 50%.
[0011] A composition for forming a coating on an optical substrate generally comprises:
[0012] - curable monomers;
[0013] - optionally one or more curable polymers;
[0014] - nanoparticles;
[0015] - black pigment; and optionally - additives.
[0016] The nanoparticles, black pigment and any additives are typically mixed with the curable monomer and any curable polymer.
[0017] The composition can be used for edge blackening of high refractive index materials or stray light control. In particular, the composition can be used for edge blackening of high refractive index materials including optical substrates.
[0018] More specifically, the invention is characterized by what is stated in the independent claims.
[0019] Considerable advantages are achieved by means of the present invention.
[0020] The compositions of the present invention exhibit properties that minimize reflection of light at the optical substrate-coating interface to provide efficient edge blackening properties. These properties are RI values that match high RI glass substrates, adjustable optical density for absorbing light within coatings of varying thicknesses while minimizing reflections due to k-value mismatches, and minimizing re-entry of light by scattering.
[0021] Typically, the cured material will have a high refractive index, for example, an RI greater than 1.75 or in the range of 1.80 to 2.3 measured at 589 nm.
[0022] By using nanoparticles as fillers, the RI can be tailored to match the RI of various substrates. The optical density, i.e. the base 10 logarithm of the reciprocal of the transmittance, can be modified by black pigments. The resin composition of the present invention allows the incorporation of nanoparticles, particularly metal oxide nanoparticles, in excess of 45% by weight of the composition.
[0023] The composition may be provided in a solvent-free form to allow for a solvent-free product.
[0024] The viscosity can be adjusted by varying the composition, particularly the relative amounts of polymer and monomer, or optionally by the use of solvents, to allow application by various contact and non-contact methods. The material is typically cured by photoactivation, particularly using ultraviolet light. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Demonstrates how a high optical density black coating reduces light reflection at the optical substrate-black coating interface;
[0026] Figure 2 shows the total reflectance of the glass coating interface for different black filler formulations; and
[0027] Figure 3 The diffuse reflectance of the glass coating interface is shown for different black filler formulations. DETAILED DESCRIPTION
[0028] It should be noted that, unless the context clearly dictates otherwise, as used herein, the singular forms "a", "an" and "the" include plural referents. It should be further understood that when the terms "comprising" and / or "including" are used in this specification, the presence of the features, steps, operations, elements and / or components is specified, but the addition of one or more other features, steps, operations, elements, components and / or groups thereof is not excluded.
[0029] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs. It should also be understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology and the present disclosure, and will not be interpreted in an idealized or overly formal sense unless explicitly defined herein.
[0030] Unless otherwise stated herein or clear from the context, any percentages mentioned herein are expressed as weight percentages based on the total weight of the corresponding composition.
[0031] Unless otherwise stated, the properties that have been experimentally measured or determined herein are measured or determined at room temperature. Room temperature is 25°C unless otherwise stated.
[0032] As used herein, the term "about" refers to a value that is ±5% of the stated value.
[0033] Unless otherwise stated, properties that have been experimentally measured or determined herein were measured or determined at atmospheric pressure.
[0034] As used herein, unless otherwise indicated, the term "average molecular weight" refers to the weight average molecular weight (also referred to as "M W ” or “MW”).
[0035] As used herein, molecular weight is measured by gel permeation chromatography using polystyrene standards.
[0036] "Particle size" and "average particle size" as referred to herein refer to the number average particle size (also referred to as "diameter") based on the largest linear dimension of the particles. It is determined by light scattering, particularly by dynamic light scattering. The average reported is the Z average, i.e., the intensity-weighted average of the hydrodynamic diameter.
[0037] As used herein, the term "average particle size" refers to the D of the cumulative volume distribution curve. 50 A value at which 50% by volume of the particles have a diameter smaller than this value.
[0038] As used herein, unless otherwise specified, the term "viscosity" refers to the dynamic viscosity at 25°C, measured by a rheometer at 2.5 s -1 The shear rate is determined.
[0039] In the present context, the term "black pigment" refers to pigments or particles having an absorption coefficient in the visible radiation range (i.e. between about 380 and 740 nm), resulting in a visually black appearance. For example, when the black pigment is present in a 50 μm thick coating at a concentration of 4%, the coating will have an optical density higher than 2.
[0040] In the present context, the term "black coating" denotes a coating which contains black pigments and has an optical density higher than 2 as measured by a spectrophotometer in the visible radiation range, ie between approximately 380 and 740 nm.
[0041] In the present context, an "optical substrate" refers to a material or a stack of materials having a high internal transmittance (above 90%) and a low attenuation level (below 10%) due to scattering or luminescence at the wavelength of light used (usually at visible wavelengths). In the present context, the optical substrate on which the coating is applied has a high refractive index, in particular, the refractive index of the optical substrate is above about 1.75, in particular above 1.8, in particular about 1.8 to 2.5, typically 1.85 to 2.3 at a wavelength of 589 nm.
[0042] The optical substrate may include: an amorphous material such as glass; a crystalline material such as a mineral crystalline material; a polymer material; or an optical coating including, for example, an inorganic filler embedded in a polymer matrix. The optical substrate may be in the form of, for example, a wafer material, and the optical substrate may consist of a single layer or a multilayer structure.
[0043] In one embodiment, the optical substrate is an optical glass, such as flint glass or crown glass. It may also contain additives, such as zinc oxide, boron oxide, barium oxide, fluorite or lead or a combination thereof.
[0044] Embodiments of the present technology provide high RI edge blackening and / or stray light control materials.
[0045] Embodiments also provide formulations that can be coated onto optical substrates, such as glass wafers, to achieve a black coating.
[0046] In an embodiment, the formulation comprises a binder such as a curable polymer, particularly a prepolymer having cross-linking groups such as a siloxane polymer, a curable monomer having cross-linking groups such as an acrylate group, or consists of or consists essentially of the same, and the binder is mixed with nanoparticles such as titanium dioxide to adjust the refractive index (RI) to match the refractive index of the optical substrate, and mixed with a black pigment such as soot or carbon black to achieve high optical density.
[0047] In an embodiment, the black coating of the present invention comprises a film formed by a photocurable composition mixed with metal oxide nanoparticles and a black pigment, and the cured solid film has a percentage of metal oxide nanoparticles greater than 45%, particularly greater than 50%, for example 55 to 90%, or 55 to 80%, calculated based on the weight of the film.
[0048] In one embodiment, the black coating comprises a film having a thickness of 1 to 300 μm. In one embodiment, the black coating comprises a film having a thickness of 5 to 100 μm, such as 10 to 50 μm. In one embodiment, the black coating comprises a film that exhibits an optical density greater than 2 at a wavelength of 400 to 740 nm at a film thickness of 50 μm.
[0049] In one embodiment, the curable monomer is selected from compounds comprising a crosslinking group. Examples of such crosslinking groups are epoxy, glycidyl, vinyl, allyl, acrylate and methacrylate, and combinations thereof.
[0050] The weight ratio between the curable polymer and the curable monomer is generally in the range of 1:100 to 100:1, such as 10:100 to 100:10, in particular 15:50 to 50:15.
[0051] In one embodiment, the nanoparticles are selected from non-absorbing metal oxide particles having a k value below 0.05 at visible wavelengths. Examples of such particles include titanium dioxide, zirconium dioxide, hafnium dioxide, germanium dioxide, aluminum oxide, barium titanate, niobium oxide, and combinations thereof.
[0052] In one embodiment, the nanoparticles are selected from metal oxide particles, such as titanium dioxide and zirconium oxide.
[0053] In one embodiment, the nanoparticles have a Z average particle size of 1 to 200 nm, in particular 2 to 100 nm.
[0054] The Z average particle size of the nanoparticles affects the viscosity and refractive index of the final formulation. Large-sized nanoparticles generally have a higher refractive index and lower viscosity than smaller-sized nanoparticles. By controlling and adjusting the viscosity, for example, by selecting the particle size of the nanoparticles, the final formulation can be adapted to different application methods, thereby obtaining a feasible formulation.
[0055] In one embodiment, the nanoparticles are generally non-aggregated.
[0056] In one embodiment, the nanoparticles are used as coated nanoparticles, and the coating is used to prevent the particles from agglomerating. Typical coatings for the nanoparticles are different silane monomers, such as methacrylate propyl trimethoxysilane, hexyl trimethoxysilane, glycidoxypropyl trimethoxysilane, or methyl trimethoxysiloxane, to name a few. The coatings for the nanoparticles can also be other oxide coatings, such as ZrO2, Al2O3, or TiO2, to further stabilize the nanoparticles from photocatalysis.
[0057] In one embodiment, the nanoparticles are provided as a undried dispersion.
[0058] In one embodiment, the weight ratio of the nanoparticles to the curable composition formed of the curable polymer and the curable monomer is 95:5 to 50:50, specifically 90:10 to 50:50, such as 85:15 to 50:50.
[0059] In one embodiment, the black pigment is selected from soot, carbon black, graphite, synthetic graphite, carbon nanotubes, metal complex dyes and metal oxide particles and combinations thereof. The black pigment may also include black organic pigments.
[0060] The concentration of black pigment in the film is selected to be from 0.1 to 20%, such as from 0.5 to 10%, calculated on the weight of curable polymer and nanoparticles, to adjust the optical density of the cured coating at the desired coating thickness.
[0061] Black pigments, such as carbon black, typically have primary particles with an average particle size of about 10 to 100 nm, while secondary particles, such as agglomerates, have a particle size of about 1 to 100 μm. Black pigments are selected to minimize light scattering by the pigment and its secondary particles, such as agglomerates.
[0062] In one embodiment, the composition comprises a non-aggregated black pigment.
[0063] In one embodiment, the film is deposited on a glass wafer, particularly a non-polished surface of a glass wafer.
[0064] In one embodiment, the film is deposited on an optical substrate or stack of optical substrates, the optical substrate or stack of optical substrates having a refractive index at 589nm greater than 1.75, or greater than 1.8, in particular 1.8 to 2.3, for example 1.80 to 2.1. In one embodiment, the film has a refractive index at 589nm of 1.80 to 2.05, or 1.90 to 2.1, or 1.95 to 2.1.
[0065] The refractive index of the film deposited on the optical substrate corresponds to or is equal to the refractive index of the optical substrate. Thus, in one embodiment, the refractive index of the film at 589 nm differs from the refractive index of the optical substrate by no more than ±0.4 units, in particular no more than ±0.1 units, in particular no more than ±0.05 units.
[0066] In one embodiment, the film coated on the planar glass wafer exhibits a reflectivity at the optical substrate-coating interface with a total reflectance to diffuse reflectance ratio greater than 10:1, particularly greater than 100:1, and typically up to 1000:1.
[0067] In one embodiment, the black pigment is selected to obtain a black coating with a diffuse reflectance below 1.5%, in particular below 1.0%.
[0068] The optical substrate typically has a thickness in the range of 100 μm to 10000 μm, for example 300 to 1500 μm.
[0069] In one embodiment, the coating film has a thickness of 5 to 100 μm, and is deposited on an optical substrate having a thickness of 100 to 1500 μm.
[0070] In one embodiment, the total reflection at the interface between the optical substrate and the coating film is less than 2%, in particular less than 1.0% at 420-740 nm.
[0071] In one embodiment, the optical substrate comprising a black coating further comprises a sheet having an edge defining a sheet, the black coating covering at least a region adjacent to the edge of the sheet.
[0072] Preferably, the sheet has a width, a length and an area, wherein the black coating covers no more than 50%, in particular no more than 25%, of the total area of the sheet. In one embodiment, the black coating comprises an integral layer extending along the width and length of the sheet, which covers 5% to 20% of the total area of the substrate adjacent to the edge of the sheet.
[0073] In one embodiment, a composition for coating an optical substrate comprises, consists of, or consists essentially of:
[0074] - up to 50 parts by weight of a curable polymer;
[0075] - up to 50 parts by weight of curable monomers;
[0076] - 50 to 100 parts by weight, for example 55 to 90 parts by weight or 55 to 85 parts by weight, of metal oxide nanoparticles; and
[0077] 0.1 to 20 parts by weight, in particular 0.5 to 10 parts by weight, of black pigments.
[0078] In the composition, the nanoparticles and the black pigment are usually mixed with the curable polymer, especially uniformly mixed with the curable polymer.
[0079] In one embodiment, the composition always includes at least some curable monomer and optionally a curable polymer.
[0080] In addition to the above components, in some embodiments, the composition further comprises a solvent capable of at least partially dissolving the curable polymer and optional monomers.
[0081] Typically, the solvent comprises 0.1 to 50% by weight of the total composition, such as 1 to 30% by mass of the total composition.
[0082] In one embodiment, a composition for coating an optical substrate comprises, consists of, or consists essentially of a mixture of:
[0083] - up to 50 parts by weight of a curable polymer;
[0084] - up to 50 parts by weight of curable monomers;
[0085] - 50 to 100 parts by weight, for example 55 to 90 parts by weight or 55 to 85 parts by weight of metal oxide nanoparticles;
[0086] - 0.1 to 20 parts by weight, in particular 0.5 to 10 parts by weight, of a black pigment; and
[0087] - 0.1 to 50%, for example 1 to 30%, calculated on the weight of the liquid composition capable of at least partially dissolving the curable polymer and optional monomers.
[0088] In one embodiment, the composition comprises a black pigment at a concentration of 0.1 to 10%, such as 0.5 to 6%, calculated based on the total weight of the composition (excluding any solvent).
[0089] In the above embodiments, there is also typically 0.1 to 25%, such as 1 to 10%, by weight of the total composition, of a photopolymerization initiator or a combination of photopolymerization initiators, as will be explained below.
[0090] In one embodiment, the composition is provided in a solvent-free or substantially solvent-free form. In particular, the composition comprises less than 5%, in particular less than 2%, of solvent, based on the total weight of the composition.
[0091] The solvent-free and solvent-containing compositions both comprise, consist of or consist essentially of 0 to 25 parts by weight (e.g., 1 to 15 parts by weight) of one or more polymers, and 5 to 50 parts by weight (e.g., 10 to 40 parts by weight) of a monomer or monomer mixture, in combination with 0.1 to 20 parts by weight of a black pigment. Typically, they also contain 0.1 to 25%, e.g., 1 to 10%, of a photopolymerization initiator, calculated based on the weight of the total composition.
[0092] In one embodiment, the curable polymer has a molecular weight (M) of 500 to 100,000 g / mol. w ). Typically, curable polymers have reactive groups which will allow the polymer to crosslink during curing.
[0093] In one embodiment, the curable polymer comprises a siloxane polymer.
[0094] To prepare a siloxane polymer, a 1 a R 2 4-a The first compound, wherein a is 1 to 3, R 1 is a reactive group, R 2 is an alkyl or aryl group. Also provided is a 3 b R 4 c R 5 4-(b+c) The second compound wherein R 3 is a cross-linking functional group, R 4 is a reactive group, R 5 is an alkyl or aryl group, and wherein b=1 to 2, and c=1 to (4-b). An optional third compound is provided with the first compound and the second compound to be polymerized therewith. An optional fourth compound may also be provided with the first compound, the second compound, and the third compound to be polymerized therewith. The third compound and the fourth compound may have the formula SiR 9 f R 10 g , where R 9 is a reactive group, and f=1 to 4, and wherein R 10 is an alkyl or aryl group, and g=4-f. If the third and fourth compounds are provided together with the first and second compounds, the third and fourth compounds are not the same. The first, second, third and fourth compounds may be provided in any order, and an oligomeric, partially polymerized form of any of these compounds may be provided in place of the above monomers.
[0095] The first compound, the second compound, the third compound, and the fourth compound, and any compounds described below, if such compounds have more than one single type of "R" group, such as multiple aryl or alkyl groups, or multiple reactive groups, or multiple crosslinking functional groups, etc., then the multiple R groups are independently selected to be the same or different at each occurrence. For example, if the first compound is SiR 1 2R 2 2, then multiple R 1 The groups are independently selected to be the same or different from each other. 2 Groups are independently selected to be the same or different from each other. Unless expressly stated otherwise, the same is true for any other compound mentioned herein.
[0096] A catalyst is also provided. The catalyst can be a base catalyst or other catalysts mentioned below. The catalyst provided should be able to polymerize the first compound and the second compound together. As mentioned above, the order of addition of the compounds and the catalyst can be any desired order. The various components provided together are polymerized to produce a siloxane polymer material with a desired molecular weight and viscosity. After polymerization, particles such as microparticles, nanoparticles or other desired particles are added, as well as other optional components such as coupling agents, catalysts, stabilizers, adhesion promoters, etc. The combination of the components of the composition can be carried out in any desired order.
[0097] More specifically, in one example, the siloxane polymer is made by polymerizing a first compound and a second compound, wherein the first compound has a chemical formula I
[0098] S i 1 a R 2 4-a I
[0099] in
[0100] a is an integer from 1 to 3,
[0101] R 1 is a reactive group, and
[0102] R 2 is an alkyl or aryl group,
[0103] and the second compound has the chemical formula II
[0104] S i 3 b R 4 c R 5 4-(b+c) II
[0105] in
[0106] R 3 is a cross-linking functional group,
[0107] R 4 is a reactive group, and
[0108] R 5 is an alkyl or aryl group, and wherein
[0109] b is an integer from 1 to 2, and c is an integer from 1 to (4-b).
[0110] The first compound may have 1 to 3 alkyl or aryl groups (R 2 ) is combined with silicon in the compound. Combinations of different alkyl groups, combinations of different aryl groups or combinations of both alkyl and aryl groups are possible. If it is an alkyl group, the alkyl group preferably contains 1 to 18, more preferably 1 to 14, and particularly preferably 1 to 12 carbon atoms. Shorter alkyl groups are envisioned, such as 1 to 6 carbon atoms (e.g., 2 to 6 carbon atoms). The alkyl group can be branched with one or more, preferably two C1 to C6 alkyl groups in the α or β position. In particular, the alkyl group is a low alkyl group containing 1 to 6 carbon atoms, which optionally carries 1 to 3 substituents selected from methyl and halogen. Methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl and tert-butyl are particularly preferred. Cycloalkyl groups are also possible, such as cyclohexyl, adamantyl, norbornene or norbornene.
[0111] If R 2 If the aryl group is an aryl group, the aryl group may be a phenyl group, which may optionally carry 1 to 5 substituents selected from halogen, alkyl or alkenyl on the ring; or a naphthyl group, which may optionally carry 1 to 11 substituents selected from halogen, alkyl or alkenyl on the ring structure, and the substituents may be optionally fluorinated (including perfluorinated or partially fluorinated). If the aryl group is a polyaromatic group, the polyaromatic group may be, for example, anthracene, naphthalene, phenanthrene, tetracene, which may optionally carry 1 to 8 substituents, or may also be optionally "spaced apart" from the silicon atom by an alkyl, alkenyl, alkynyl or aryl group containing 1 to 12 carbons. Monocyclic structures such as phenyl groups may also be spaced apart from the silicon atom in this manner.
[0112] The siloxane polymer is prepared by a polymerization reaction, preferably a base-catalyzed polymerization reaction, between a first compound and a second compound. Optional additional compounds may be included as part of the polymerization reaction as described below.
[0113] The first compound may have any suitable reactive group R 1, such as hydroxyl, halogen, alkoxy, carboxyl, amine or acyloxy. For example, if the reactive group in the first compound is an -OH group, more specific examples of the first compound may include silanediols, such as diphenylsilanediol, dimethylsilanediol, diisopropylsilanediol, di-n-propylpropylene glycol, di-n-butylsilanediol, di-tert-butylsilanediol, diisobutylsilanediol, phenylmethylsilanediol and dicyclohexylsilanediol.
[0114] The second compound may have any suitable reactive group R 4 , such as hydroxyl, halogen, alkoxy, carboxyl, amine or acyloxy, which can be the same as or different from the reactive group in the first compound. In one example, the reactive group is not -H in the first compound or the second compound (or any compound participating in the polymerization reaction to form the siloxane polymer, such as the third compound, etc.), so that the resulting siloxane polymer does not have any or substantially any H groups directly bonded to Si in the siloxane polymer. The group R 5 , if present in the second compound, is independently an alkyl or aryl group, such as the group R in the first compound 2 . Alkyl or aryl R 5 can be combined with the group R in the first compound 2 Same or different.
[0115] The cross-linking reactive group R of the second compound 3 It can be any functional group that can be crosslinked by acid, base, free radical or thermal catalytic reaction. These functional groups can be, for example, any epoxide, oxetane, acrylate, alkenyl, alkynyl or thiol group.
[0116] If an epoxide group, it may be a cyclic ether having three ring atoms, which can be crosslinked using acid, base, and heat catalyzed reactions. Examples of these epoxide-containing crosslinking groups are glycidyloxypropyl and (3,4-epoxycyclohexyl)ethyl, to name a few.
[0117] In the case of an oxetane group, it may be a cyclic ether having four ring atoms which can be crosslinked by acid, base and heat catalyzed reactions. Examples of such oxetane-containing silanes include 3-(3-ethyl-3-oxetanylmethoxy)propyltriethoxysilane, 3-(3-methyl-3-oxetanylmethoxy)propyltriethoxysilane, 3-(3-ethyl-3-oxetanylmethoxy)propyltrimethoxysilane or 3-(3-methyl-3-oxetanylmethoxy)propyltrimethoxysilane, to name a few.
[0118] If an acrylate group, it can be an acrylate or methacrylate, which can be crosslinked using a free radical initiator that can be activated by UV light or heat. Examples of such acrylate-containing silanes are 3-(trimethoxysilyl)propyl methacrylate, 3-(trimethoxysilyl)propyl-acrylate, 3-(triethoxysilyl)propyl methacrylate, 3-(triethoxysilyl)propyl acrylate, 3-(dimethoxymethylsilyl)propyl methacrylate or 3-(methoxydimethylsilyl)propyl methacrylate, to name a few.
[0119] If alkenyl, such groups may have preferably 2 to 18, more preferably 2 to 14 and particularly preferably 2 to 12 carbon atoms. The vinyl group, i.e. the two carbon atoms bonded via a double bond, is preferably located at position 2 or higher in the molecule relative to the Si atom. Branched alkenyl groups are preferably branched in the α or β position with one and more, preferably two, C1 to C6 alkyl, alkenyl or alkynyl groups, optionally fluorinated or perfluorinated alkyl, alkenyl or alkynyl groups.
[0120] If alkynyl, it may have preferably 2 to 18, more preferably 2 to 14 and particularly preferably 2 to 12 carbon atoms. The ethynyl group, i.e. the two carbon atoms bonded by a triple bond, is preferably located at position 2 or higher in the molecule relative to the Si or M atom. The branched alkynyl group is preferably branched in the α or β position with one and more, preferably two, C1 to C6 alkyl, alkenyl or alkynyl groups, optionally perfluorinated alkyl, alkenyl or alkynyl groups.
[0121] If a thiol group, it may be any organosulfur compound containing a carbon-bonded mercapto group. Examples of thiol-containing silanes are 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
[0122] The reactive group in the second compound can be an alkoxyl group. The alkyl residue of the alkoxyl group can be straight or branched. Preferably, the alkoxyl group is composed of a lower alkoxyl group with 1 to 6 carbon atoms, such as methoxy, ethoxy, propoxy and tert-butoxy. The specific example of the second compound is a silane, such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-(trimethoxysilyl)propylmethacrylate, 3-(trimethoxysilyl)propylacrylate, (3-glycidyloxypropyl)trimethoxysilane or 3-glycidyloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane etc.
[0123] The third compound and the fourth compound may be provided together with the first compound and the second compound to be polymerized therewith. The third compound and the fourth compound may independently have a chemical formula III
[0124] S i 9 f R 10 g III
[0125] in
[0126] R 9 is a reactive group, and
[0127] f = 1 to 4, and wherein
[0128] R 10 is an alkyl or aryl group, and
[0129] g=4-f.
[0130] One such example is tetramethoxysilane. Other examples include phenylmethyldimethoxysilane, trimethylmethoxysilane, dimethyldimethoxysilanesilane, vinyltrimethoxysilane, allyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, propylethyltrimethoxysilane, phenylmethyldiethoxysilane, trimethylethoxysilane, dimethyldiethoxysilanesilane, vinyltriethoxysilane, allyltriethoxysilane, methyltriethoxysilane, methyltripropoxysilane, propylethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and the like.
[0131] If a fourth compound is provided with the first compound, the second compound, and the third compound, the fourth compound is different from the third compound.
[0132] Although the polymerization of the first compound and the second compound can be carried out using an acid catalyst, a base catalyst is preferred. The base catalyst used in the base-catalyzed polymerization between the first compound and the second compound can be any suitable basic compound. Examples of these basic compounds are any amine, such as triethylamine; and any barium hydroxide, such as barium hydroxide, barium hydroxide monohydrate, barium hydroxide octahydrate, etc. Other basic catalysts include magnesium oxide, calcium oxide, barium oxide, ammonia, ammonium perchlorate, sodium hydroxide, potassium hydroxide, imidazolone or n-butylamine. In a specific example, the base catalyst is Ba(OH)2. Relative to the first compound and the second compound, the base catalyst can be provided together in a weight percentage of less than 0.5% or in a lower amount (such as a weight percentage of less than 0.1%).
[0133] The polymerization can be carried out in the melt phase or in a liquid medium. The temperature is in the range of about 20 to 200°C, typically about 25 to 160°C, and in particular about 40 to 120°C. Typically, the polymerization is carried out at ambient pressure, with the maximum temperature being determined by the boiling point of any solvent used. The polymerization can be carried out under reflux conditions. Other pressures and temperatures are also possible. The molar ratio of the first compound to the second compound can be 95:5 to 5:95, in particular 90:10 to 10:90, preferably 80:20 to 20:80. In a preferred example, the molar ratio of the first compound to the second compound (or the second compound plus other compounds participating in the polymerization reaction - see below) is at least 40:60, or even 45:55 or more.
[0134] In one example, the first compound has -OH groups as reactive groups and the second compound has alkoxy groups as reactive groups. Preferably, for the amount of the first compound added, the total number of -OH groups does not exceed the total number of reactive groups (e.g., alkoxy groups in the second compound), and is preferably less than the total number of reactive groups in the second compound (or the second compound plus any other compound with added alkoxy groups, such as added tetramethoxysilane or other third compound participating in the polymerization reaction, such as mentioned herein). When the number of alkoxy groups exceeds the hydroxyl groups, all or substantially all of the -OH groups will react and be removed from the siloxane, such as methanol if the alkoxysilane is methoxysilane, ethanol if the alkoxysilane is ethoxysilane, etc. Although the number of -OH groups in the first compound and the number of reactive groups (preferably different from -OH groups) in the second compound can be substantially the same, it is preferred that the total number of reactive groups in the second compound is more than 10%, preferably more than 25%, than the -OH groups in the first compound. In some embodiments, the number of reactive groups of the second compound is more than 40%, even more than 60%, more than 75%, or up to more than 100% more than the -OH groups of the first compound. Depending on the selected compound, methanol, ethanol or other byproducts of the polymerization reaction are removed after polymerization, preferably evaporated in a drying chamber.
[0135] The siloxane polymer is first provided in the form of a prepolymer having a weight average molecular weight of 500 to 5,000 g / mol, such as 750 to 3,000 g / mol.
[0136] After curing, molecular weights are typically as high as 200,000 g / mol.
[0137] In a specific embodiment, the curable polymer has a molecular weight (M) of 500 to 2500 g / mol. w), the siloxane prepolymer preferably having one or more reactive groups, the one or more reactive groups being particularly selected from epoxy, glycidyl, vinyl, allyl, acrylate and methacrylate and combinations thereof.
[0138] In one embodiment, the curable monomer is selected from compounds having crosslinkable reactive groups such as epoxy, glycidyl, vinyl, allyl, acrylate, and methacrylate, and combinations thereof.
[0139] Examples of these monomers are methyl acrylate, ethyl acrylate, 2-ethylhexyl (meth)acrylate, hydroxyethyl (meth)acrylate, butyl (meth)acrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, vinyl diacrylate, tetra(ethylene glycol) diacrylate, ethyl 2-cyanoacrylate, 2-hydroxyethyl acrylate, isobornyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl acrylate, 2-carboxyethyl acrylate, trimethylolpropane (EO)n triacrylate, caprolactone acrylate, polypropylene glycol monomethacrylate, cyclic trimethylolpropane formal acrylate, phenoxybenzyl acrylate, and the like. acrylate, 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, o-phenylphenol EO acrylate, 4-tert-butylcyclohexyl acrylate, benzyl acrylate, benzyl methacrylate, biphenyl methacrylate, lauryl acrylate, lauryl methacrylate, tridecyl acrylate, lauryl tetradecyl methacrylate, isodecyl acrylate, isodecyl methacrylate, phenol (EO) acrylate, phenoxyethyl methacrylate, phenol (EO) 2 acrylate, phenol (EO) 4 acrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, nonylphenol (PO) 2 acrylate, nonylphenol ( EO)4 acrylate, nonylphenol (EO)8 acrylate, ethoxyethoxyethyl acrylate, stearyl acrylate, stearyl methacrylate, methoxy PEG600 methacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, 1,6-hexanediol (EO)n diacrylate, polypropylene glycol 400 diacrylate, 1,4-butanediol dimethacrylate, polypropylene glycol 700 (EO)6-dimethacrylate, 1,6-hexanediol (EO)n diacrylate, hydroxyvitamin neopentyl glycol diacrylate, bisphenol A (EO)10-diacrylate, bisphenol A(EO)10-dimethacrylate, neopentyl glycol dimethacrylate, neopentyl glycol (PO)2 diacrylate, tripropylene glycol diacrylate, ethylene glycol dimethacrylate, dipropylene glycol diacrylate, bisphenol A(EO)30 diacrylate, bisphenol A(EO)30-dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, bisphenol A(EO)4 diacrylate, bisphenol A(EO)4-dimethacrylate, bisphenol A(EO)3-diacrylate, bisphenol A(EO)3-dimethacrylate, 1,3-Butanediol dimethacrylate, tricyclodecane dimethanol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol 400 diacrylate, polyethylene glycol 400 dimethacrylate, polyethylene glycol 200 diacrylate, polyethylene glycol 200 dimethacrylate, polyethylene glycol 300 diacrylate, polyethylene glycol 600 diacrylate, polyethylene glycol 600 dimethacrylate, bisphenol F (EO) 4 diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, trimethylolpropane (EO) 3-triacrylate Acrylates, trimethylolpropane (EO) 15-triacrylate, trimethylolpropane (EO) 6 triacrylate, trimethylolpropane (EO) 9-triacrylate, glycerol (PO) 3 triacrylate, pentaerythritol triacrylate, trimethylolpropane (PO) 3 triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, pentaerythritol (EO) n tetraacrylate, di(trimethylol)propane tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, to name a few. ,
[0140] In one embodiment, the curable polymers and monomers are cured by free radical curing.
[0141] Typically, monomers and polymers can be cured by photopolymerization using active energy rays such as visible light, electron beams, and particularly ultraviolet (UV) rays.
[0142] In embodiments of the present technology, the composition further comprises at least one photopolymerization initiator, and optionally a co-initiator, such as a spectral sensitizer, and optionally a reducing agent.
[0143] In one embodiment, the composition comprises a photopolymerization initiator or a combination thereof, particularly a UV initiator or a combination of UV initiators, for achieving curing of the curable polymer. Examples of photopolymerization and UV initiators include the following: carbonyl compounds, such as aromatic ketones; acylphosphine oxide compounds; aromatic onium salt compounds; organic peroxides; thio compounds; hexaarylbisimidazoles; ketoxime esters; borate compounds, azinium compounds; and metallocene compounds, active ester compounds, and alkylamine compounds.
[0144] In one embodiment, a ketoxime ester is used as a photopolymerization initiator.
[0145] Typically, the photopolymerization or UV initiator is present in an amount of 0.1 to 25 wt %, in particular 0.5 to 20 wt %, such as 0.5 to 10 wt %, of the composition.
[0146] The composition preferably comprises additives capable of adjusting the properties of the composition. Such additives are selected from the group of additives capable of adjusting the wettability, adhesion, thixotropy, foaming properties and combinations thereof of the composition. Typically, the concentration of the additive is 0.01 to 15%, in particular about 0.1 to 10%, of the total weight of the composition (including any solvent).
[0147] In one embodiment, the composition comprises a solvent for the curable polymer. The solvent may optionally be selected so that it is also capable of dissolving the black pigment (particularly when an organic black pigment is used).
[0148] In one embodiment, the solvent primarily dissolves the curable polymer, while the nanoparticles and black pigment are dispersed in the liquid phase rather than dissolved therein.
[0149] The dynamic viscosity of the composition at 25° is generally in the range of 5 mPas-1,000,000 mPas or 5 mPas-500,000 mPas, for example about 50 to 50,000 mPas or about 100 to 200,000 mPas, in particular 200 to 100,000 mPas, such as 250 to 10,000 mPas (measured by a rheometer at 2.5 s -1 shear rate determination).
[0150] For application, the viscosity of the composition can be adjusted, for example, by adjusting the solid content of the composition. Typically, the solid content is in the range of 10% to 100% by weight of the total composition, particularly about 30% to 100% by weight, such as 40% to 100% by weight, or 60% to 100% by weight, particularly 80% to 100% by weight.
[0151] In one embodiment, the viscosity of the composition is adjusted by adjusting the amount of solvent for the curable polymer. Thus, the viscosity can be adjusted by adding 10 to 200 parts by weight of a liquid capable of dissolving the curable polymer to 100 parts by weight of a solid formed by the polymer, nanoparticles and black pigment.
[0152] The solvent is, for example, selected from the group of organic solvents such as ketones, ethers, alcohols and esters. As specific examples, the following can be mentioned: acetone, tetrahydrofuran (THF), toluene, methanol, ethanol, 2-propanol, propylene glycol monomethyl ether, methyl tert-butyl ether (MTBE), propylene glycol propyl ether, propylene glycol propyl ether (PnP), propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether PGME.
[0153] In one embodiment, propylene glycol monomethyl ether acetate (abbreviated as "PGMEA") is used.
[0154] In one embodiment, the viscosity of the composition is adjusted by adjusting the amount of monomer. This allows a solvent-free composition with a predetermined viscosity to be provided. More specifically, in one embodiment, 50 to 100% of the curable components of the coating are provided by the monomers in the composition, the percentage being calculated based on the total weight of the curable components (particularly the polymer and the monomer).
[0155] In one embodiment, for compositions used to produce coatings having an RI of 1.9 or greater, 80 to 100% of the curable components of the coating are provided by the monomers in the composition.
[0156] In one embodiment, a composition for a coating of an optical substrate is provided by the following steps:
[0157] - adding metal oxide nanoparticles to the curable monomer and any curable polymer in the liquid phase to provide a mixture,
[0158] - evaporating at least part or all of the liquid phase, and
[0159] - Add black pigment, curing catalyst and additives to the mixture.
[0160] After evaporation of the solvent, the mixture of polymer, monomer, and nanoparticles is typically a viscous fluid or syrup.
[0161] In one embodiment, the black pigment is added to a mixture formed from the other components to form a modified mixture, which is then milled to disperse or dissolve the black pigment.
[0162] In one embodiment, during preparation of the composition, aggregation of the black pigment is prevented.
[0163] The composition can be applied to the surface of the substrate by a variety of coating methods.
[0164] In one embodiment, the coating method is selected from the group consisting of contactless or contact methods, in particular from the group consisting of spot coating, spray coating, slot coating, spin coating, doctor blade coating, curtain coating, contactless or contact painting and printing, such as flexographic printing or screen printing.
[0165] The composition is then cured by photocuring it using, for example, UV light to form a cured film. Thus, the polymer and monomer are cured and form a cross-linked network on the surface. This polymer matrix adheres to the surface and binds the nanoparticles and black pigment to the surface.
[0166] The UV light used to achieve photocuring generally exhibits a peak in the range of 250nm to 450nm. When a single-wavelength UV light source (such as an LED) is used, the wavelength is generally selected from one or more of the following: 285nm, 300nm, 310nm, 365nm, 385nm, 395nm and 405nm. According to one embodiment, the energy dose of the UV light is 1 to 500J / cm 2 , such as 5 to 100 J / cm 2 , for example 10 to 50 J / cm 2 within the range.
[0167] In one embodiment, the composition is used for high refractive index edge blackening of a high refractive index material. Typically, the high refractive index material comprises a glass substrate, in particular a glass substrate having an unpolished rough surface, and the composition is coated on the unpolished rough surface.
[0168] By applying the composition in a solvent-free form, no or substantially no solvent evaporates during curing. Thus, a uniform film is formed on the surface, which allows the nanoparticles and black pigment to be evenly distributed on the surface.
[0169] The following non-limiting examples illustrate some embodiments.
[0170] Example
[0171] Synthesis of Siloxane Polymers:
[0172] A 500 mL round bottom flask with a stirring bar and a reflux condenser was charged with diphenylsilanediol (60 g, 45 mol %), [3-(methacryloyloxy)propyl]trimethoxysilane (55.12 g, 36.7 mol %) and tetramethoxysilane (17.20 g, 18.3 mol %). The flask was heated to 80° C. under a nitrogen atmosphere and 0.08 g of barium hydroxide monohydrate dissolved in 1 mL of methanol was added dropwise to the silane mixture. The silane mixture was stirred at 80° C. for 30 minutes, during which time the diphenylsilanediol reacted with the alkoxysilane. After 30 minutes, the methanol formed was evaporated under vacuum. The viscosity of the siloxane polymer was 1200 mPas and the molecular weight (M w ) is 1200g / mol.
[0173] Formation of the composition:
[0174] The siloxane polymer of the previous step is mixed with a curable monomer and a TiO2 nanoparticle solution in PGMEA to achieve a predetermined ratio between the polymer and the nanoparticles. The solvent is evaporated off under vacuum using a rotary evaporator, a curing catalyst, additives and a black absorptive pigment are added, and the preparation is thoroughly mixed. Finally, the composition is ground using a three-roll mill to obtain a uniform mixture.
[0175] Six different formulations (Formulations 1-6) were prepared with three different nanoparticle loadings and two TiO2 nanoparticle types (nanoparticle A with a Z-average of 37 nm and nanoparticle B with a Z-average of 81 nm). The compositions in weight percent are mentioned in Table 1.
[0176] The refractive index of the formulation was measured from the formulation before the addition of the black absorbing pigment. Samples of the siloxane polymer and nanoparticle solutions were spin-coated on silicon wafers and exposed to UV light via a 405 nm UV-LED and 20 J / cm 2 The refractive index was measured at a wavelength of 589 nm using an ellipsometer (Woollam alpha-SE). The viscosity of the final formulation was measured at a shear rate of 10 1 / s using a rheometer.
[0177] Table 1
[0178]
[0179] The results show that the particle size of TiO2 is very important in controlling the viscosity and refractive index of the formulation in the solvent-free state. Formulations with smaller TiO2 particle sizes have higher viscosities than formulations with larger particle sizes. In the case of the highest nanoparticle loading (Formulations 3 and 6), the smaller nanoparticle formulations are dry and the viscosity cannot even be measured.
[0180] Another finding is the refractive index of the formulation. Larger particle size TiO2 nanoparticles produce a higher refractive index compared to the same formulation with smaller particle size nanoparticles. In the formulation, small particle size is favored due to lower scattering cross section, resulting in better performance. Scattering by large nanoparticles produces diffuse reflectivity, which increases the reflectivity at the optical substrate-coating interface.
[0181] Another group of compositions is made by changing the black pigment / filler used. Preparations 7 to 11 were prepared similarly to Preparation 1, but the pigment type / filler was changed. Three different carbon black powders were tested: Kremerpigment's furnace black 47250, Mitsubishi Chemical Corporation's MA11 carbon black (average particle size 29nm), and Cabot's M1100 carbon black (surface treated to improve dispersibility). A black pigment X55 from BASF was tested, and a PGMEA dispersion of MA11 (total solid content of 20%) was made by rock grinding MA11 with 30% by weight of PX4310 manufactured by Efka in a PGMEA solution. For the MA11 dispersion, carbon black was added before the solvent evaporation step to remove excess PGMEA from the dispersion. The composition of preparations 7 to 11 by weight percentage is shown in Table 2.
[0182] Table 2
[0183] Components Preparation 7 Preparation 8 Preparation 9 Preparation 10 Preparation 11 Siloxane polymer 9 9 9 9 9 <![CDATA[Average value of AZ of TiO2 nanoparticles: 36 nm]]> 56 56 56 56 56 Monomer Biphenyl Methacrylate 21 21 21 21 21 Additive Hydroxyethyl Methacrylate 8 8 8 8 8 Furnace Black 47250 2 0 0 0 0 Mitsubishi MA11 0 2 0 0 0 Cabot M1100 0 0 2 0 0 Mitsubishi MA11-PGMEA dispersion 0 0 0 2 0 X55 black pigment 0 0 0 0 2 Initiator OXE-02 4 4 4 4 4
[0184] For reflectivity studies, the formulations were coated as 60 μm layers on high RI glass substrates (RI 1.8, 589 nm) by doctor blade. After coating the film, a 405 nm UV-LED was used at 20 J / cm 2 The film is cured by UV. The cured formulation forms a reflective smooth black surface on air surfaces.
[0185] The functionality of the formulations as edge blackening materials was shown by measuring the reflectance of the interface between the high refractive index glass and formulations 7 to 11. The reflectance was measured using a Konica Minolta CM-3600A spectrophotometer, which utilizes an integrating sphere and can measure both diffuse and total reflectance. The incident angle of the light was 8°. The sample was placed on the device with the uncoated glass side facing the light beam. It should be noted that in this setup, it is impossible to measure the reflectance of the glass-coating interface without the reflectance from the air-glass interface, which is why a correction for this reflection was made from the reflectance data, as shown below.
[0186] First, measure the reflectivity of the clean substrate. Assume that the reflectivity R of the substrate has only a specular component. The clean substrate has two identical surfaces with a reflectivity of r1, so the measured reflectivity can be approximated as the result of the following reflectivity:
[0187]
[0188] The single interface reflectivity is calculated using the previous equation based on the measured substrate data.
[0189] Based on the reflectivity of the air-glass interface, r1, and the reflectivity of the glass-coating interface, r2, the reflectivity of the sample coating can be approximated as
[0190] R 样品 =r1+r2·(1-r1) 2 .
[0191]
[0192] Multiply the measured diffuse reflection component by a simplified correction factor (1-r1) -2 , this simplified correction factor corrects for both the intensity loss of incident light at the air-glass interface and the reflection of scattered light at the glass-air interface. The correction for the reflection of scattered light is simplified by using the same reflectivity of the air-glass interface as measured for an 8° incident angle, which underestimates the correction.
[0193] The calculated reflectivity value of the glass-coating interface, r2, is as follows Figure 2 (total reflectance) and Figure 3 The reference value for uncoated glass is the reflectivity r1.
[0194] The results show that black pigment / filler has a large impact on total reflectance, especially diffuse reflectance, which is included in the total reflectance value. This shows how much the scattering caused by the black pigment filler affects the performance of the edge blackening material. The measurements show that the diffuse reflectance accounts for the majority of the total reflectance when the refractive index difference is minimal.
[0195] The lowest total and specular reflectances were obtained with the X55 black pigment dissolved into the resin system, and therefore, the scattering from the black pigment was very low. The Cabot M1100 carbon black, which was surface treated to improve dispersibility, obtained the second lowest total and specular reflectances. Mitsubishi MA11 showed a clear improvement in diffuse reflectance when the carbon black was dispersed in PGMEA using a dispersant, but in terms of total reflectance, the results were higher than those of MA11 used as a powder. Untreated high particle size carbon black 47250, where light scattering between the resin and the black filler may be large, obtained higher reflectances.
Claims
1. Black coating, including: - A film formed from a photocurable composition mixed with metal oxide nanoparticles and a black pigment, the cured solid film having a weight percentage of metal oxide nanoparticles higher than 45%.
2. The black coating of claim 1, wherein the film has a refractive index greater than 1.75, the refractive index measured at 589 nm.
3. The black coating according to claim 1 or 2, wherein the film has a thickness of 1 to 300 μm.
4. A black coating according to any one of the preceding claims, wherein the film has an optical density exceeding 2 between wavelengths of 400 and 740 nm.
5. A black coating according to any one of the preceding claims, wherein the nanoparticles are selected from non-absorbing metal oxide particles, such as titanium dioxide, zirconium dioxide, hafnium dioxide, aluminum oxide, germanium dioxide, barium titanate, niobium oxide and combinations thereof, and the non-absorbing metal oxide particles have a Z average particle size of 1 to 200 nm, in particular 2 to 100 nm.
6. A black coating according to any one of the preceding claims, wherein the black coating has a refractive index, wherein the complex part of the refractive index is below 0.
05.
7. A black coating according to any one of the preceding claims, wherein the weight ratio of nanoparticles to curable components is from 95:5 to 50:50, in particular from 90:10 to 50:50, for example from 85:15 to 50:
50.
8. The black coating according to any one of the preceding claims, wherein the black pigment is selected from soot, carbon black, carbon nanotubes, graphite, organic pigments, metal complex dyes and metal oxide particles and combinations thereof.
9. A black coating according to any one of the preceding claims, wherein the black pigment is selected to obtain a black coating with a diffuse reflectance below 1.5%, in particular below 1.0%.
10. A black coating according to any one of the preceding claims, wherein the film is located on an optical substrate, the refractive index of the film is equal to the refractive index of the optical substrate, in particular, the refractive index of the film differs from the refractive index of the optical substrate by no more than ±0.4 units, in particular no more than ±0.1 units, in particular no more than ±0.05 units, the refractive index being measured at 589 nm.
11. A black coating according to any one of the preceding claims, wherein the film is deposited on an optical substrate or a stack of optical substrates having a refractive index greater than 1.75, in particular greater than 1.
80.
12. A black coating according to any one of the preceding claims, wherein the total reflection at the interface between the optical substrate and the coating film is less than 2% at 400-740 nm.
13. A black coating according to any one of the preceding claims, wherein the composition is cured by ultraviolet light.
14. A black coating according to any one of the preceding claims, wherein the composition comprises: - 0 to 50 parts by weight of a curable polymer; - monomers in an amount of up to 50 parts by weight; - 50 to 100 parts by weight of nanoparticles; and - 0.1 to 20 parts by weight, in particular 0.5 to 5 parts by weight, of a black pigment; The nanoparticles and black pigment are mixed with the curable polymer and curable monomer.
15. A black coating according to any one of the preceding claims, wherein - the curable polymer, if any, has one or more reactive groups, in particular selected from epoxy, glycidyl, vinyl, allyl, acrylate and methacrylate, and combinations thereof, and preferably comprises a molecular weight (M w ) is a prepolymer of 500 to 2500 g / mol; and - The curable monomer is selected from compounds having crosslinkable reactive groups such as epoxy, glycidyl, vinyl, allyl, acrylate and methacrylate, and combinations thereof.
16. A composition for a cured solid coating of an optical substrate, comprising: - 0 to 50 parts by weight of a curable polymer; - monomers in an amount of up to 50 parts by weight; - 50 to 100 parts by weight of nanoparticles; and - 0.1 to 20 parts by weight of black pigment; The nanoparticles and black pigment are mixed with the curable polymer and curable monomer.
17. The composition according to claim 16, wherein the curable polymer is selected from a group consisting of polymers having a molecular weight (M) of 500 to 100,000 g / mol. w ) and having one or more reactive groups selected from epoxy, glycidyl, vinyl, allyl, acrylate, hydride, thiol and methacrylate, and combinations thereof.
18. The composition of claim 16 or 17, wherein the curable monomer has one or more reactive groups selected from epoxy, glycidyl, vinyl, allyl, acrylate, hydride, thiol and methacrylate, and combinations thereof.
19. The composition according to claims 16 to 18, wherein the nanoparticles are selected from metal oxide particles such as titanium dioxide, zirconium dioxide, hafnium dioxide, aluminum oxide, germanium dioxide, barium titanate, niobium oxide and combinations thereof, the metal oxide particles having a Z average particle size of 1 to 200 nm, in particular 2 to 100 nm.
20. The composition according to any one of claims 16 to 19, wherein the weight ratio of nanoparticles to curable component is from 95:5 to 50:50, in particular from 90:10 to 50:50, such as from 85:15 to 50:
50.
21. A composition according to any one of claims 16 to 20 comprising a black pigment in a concentration of 0.1 to 10%, such as 0.5 to 6%, calculated on the total weight of the composition excluding solvent.
22. A composition according to any one of claims 16 to 21 comprising a solvent for varying the viscosity of the composition, the solvent optionally also being capable of dissolving the black pigment.
23. The composition according to any one of claims 16 to 22, wherein the solids content of the composition is 60 to 100% by weight, in particular 80 to 100% by weight, the remainder comprising solvent.
24. A composition according to any one of claims 16 to 23, comprising from 0.1 to 25%, such as from 1 to 10%, of a photopolymerisation initiator or a combination of photopolymerisation initiators, based on the total weight of the composition.
25. The composition according to any one of claims 16 to 24, comprising additives capable of adjusting the properties of the composition selected from the group consisting of wettability, adhesion, thixotropy, foaming and combinations thereof.
26. The composition according to any one of claims 16 to 25, wherein the rheometer is used to measure the -1 The composition has a dynamic viscosity of 5 mPas to 1,000,000 mPas, such as about 50 to 50,000 mPas.
27. A composition according to any one of claims 16 to 26, comprising: - up to 50 parts by weight, in particular 1 to 15 parts by weight, of a curable polymer; - up to 50 parts by weight, in particular from 10 to 40 parts by weight, of a curable monomer; - 50 to 100 parts by weight of nanoparticles; - 0.1 to 20 parts by weight, in particular 0.5 to 5 parts by weight, of a black pigment; and optionally - 0.1 to 50%, in particular 1 to 30%, of a solvent, calculated on the total weight of the composition.
28. A composition according to any one of claims 16 to 27 comprising less than 5% solvent, calculated on the total weight of the composition.
29. An optical substrate comprising a black coating according to any one of claims 1 to 15.
30. An optical substrate according to claim 29, comprising a sheet having an edge defining a sheet, the black coating covering at least an area adjacent to the edge of the sheet.
31. An optical substrate according to claim 29 or 30, comprising a sheet having a width, a length and an area, wherein the black coating covers no more than 50%, in particular no more than 25%, of the total area of the sheet.
32. An optical substrate according to any one of claims 29 to 31, wherein the black coating comprises an integral layer extending along the width and the length of the sheet, the integral layer covering 5% to 20% of the total area of the substrate adjacent the edge of the sheet.
33. Use of the composition according to any one of claims 16 to 28 for blackening of high refractive index edges of high refractive index materials or for stray light control.
34. The use according to claim 33, wherein the high refractive index material comprises an optical substrate, in particular a glass substrate, and the composition is coated on the optical substrate, in particular a glass substrate.
Citation Information
Patent Citations
Black type ink composition for ink-jet printing, light-shielding film, optical member, and method for forming image
CN111886302A
Optical element, light-shielding coating material set, and method for manufacturing optical element
US20160282612A1