Sputtering target, method for producing sputtering target, oxide thin film, thin film transistor, and electronic device

By using an oxide sintered body sputtering target with specific composition and density, the film formation process of oxide thin films can be controlled, solving the uniformity problem of amorphous thin films on large-area substrates and improving the processability and film quality of thin film transistors.

CN118922581APending Publication Date: 2024-11-08IDEMITSU KOSAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029265.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-29
Filing Date
2023-03-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies make it difficult to uniformly deposit amorphous indium oxide thin films on large-area substrates, which reduces the processability of the films and affects the manufacturing process of thin-film transistors.

Method used

An oxide sintered sputtering target with a hydrogen concentration of 5×10¹⁶ atoms/cm³ or higher, an In to O atomic concentration ratio of 1.3 or higher and less than 2.5, and a density of 6.0 g/cm³ or higher is used. The oxide film formation process is controlled by cooling treatment in an atmosphere containing inert gas and hydrogen.

Benefits of technology

This method achieves uniform amorphization of oxide thin films on large-area substrates, improves the processability and film quality of thin-film transistors, reduces residues in patterning processes, and enhances the manufacturing efficiency of TFTs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922581A_ABST
    Figure CN118922581A_ABST
Patent Text Reader

Abstract

A sputtering target is provided with an oxide sintered body containing indium oxide as a main component. The oxide sintered body has a hydrogen content of 5 * 1016 atoms / cm3 or more, an atomic concentration ratio of an I n (indium) element to an O (oxygen) element (O element / I n element) of 1.3 or more and less than 2.5, and a density of 6.0 g / cm3 or more as measured by the Archimedes method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sputtering target, a method for manufacturing the sputtering target, an oxide film, a thin film transistor and an electronic device. Background Art

[0002] In recent years, research has been conducted on using a crystalline oxide semiconductor thin film as a channel layer of a thin film transistor (hereinafter, sometimes referred to as a TFT).

[0003] In order to apply a crystalline oxide semiconductor thin film to a channel layer of a TFT, a method of sputtering a sputtering target having a sintered body having the same atomic composition as that of the crystalline oxide semiconductor thin film may be mentioned.

[0004] If the film is crystallized just after sputtering, the processability of the crystalline oxide semiconductor in an acid solution such as an organic acid is reduced, making it difficult to apply to TFT. Therefore, the oxide film is formed in an amorphous state just after sputtering, and the film is crystallized by annealing after film formation. A crystalline oxide semiconductor film with less (or no) added elements such as indium oxide can be obtained by introducing hydrogen during sputtering and precisely controlling the hydrogen flow rate to suppress the atomic diffusion rate.

[0005] For example, Patent Document 1 describes a thin film transistor having a source electrode, a drain electrode, a gate electrode, a gate insulating film, and a channel layer composed of an oxide semiconductor. In the thin film transistor described in Patent Document 1, the average carrier concentration of the channel layer is 1×10 16 / cm 3 ~5×10 19 / cm 3 In the range of, there is a carrier concentration region higher than the average carrier concentration on the gate insulating film side of the channel layer, and the channel layer has substantially the same composition. In addition, in the thin film transistor described in Patent Document 1, it is described that the oxide semiconductor preferably has a crystalline structure.

[0006] Patent Document 2 describes a sputtering target composed of an oxide sintered body containing indium oxide as a main component. Regarding the sputtering target described in Patent Document 2, the Archimedean density AD (g / cm 3 ) and the theoretical density TD (g / cm 3 ) is in the relationship of AD / TD>0.995.

[0007] Patent Document 3 describes an indium oxide-based sputtering target, which is characterized in that it is a sintered body substantially composed of indium and oxygen and has a relative density of 90% or more.

[0008] Patent Document 4 describes an indium oxide target composed of an indium oxide sintered body, wherein the indium oxide sintered body is composed of In and O elements, has a relative density of more than 90%, a residual stress x of -200 ≤ x ≤ 200 MPa, and a volume of 1.0×10 4 mm 3 As above, they are integrally formed.

[0009] Patent Document 5 describes a sputtering target for forming an oxide semiconductor film. The hydrogen concentration of the sputtering target is less than 1×10 16 atoms / cm 3 .

[0010] Non-patent document 1 describes a high-mobility hydrogenated polycrystalline In2O3 (In2O3:H) thin film transistor using a low-temperature solid phase crystallization (SPC) process, in which an amorphous In2O3:H thin film is obtained by introducing hydrogen during sputtering film formation, and the In2O3:H thin film is crystallized by subsequent annealing treatment.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: International Publication No. 2013 / 021632

[0014] Patent Document 2: Japanese Patent Application Publication No. 2005-060798

[0015] Patent Document 3: Japanese Patent Application Laid-Open No. 9-125236

[0016] Patent Document 4: Japanese Patent Application Laid-Open No. 8-013140

[0017] Patent Document 5: Japanese Patent Application Publication No. 2015-061953

[0018] Non-patent literature

[0019] Non-patent document 1: Magari, Y., Kataoka, T., Yeh, W., & Furuta, M. (2022). High-mobility hydrogenated polycrystalline In2O3 (In2O3: H) thin-film transistors. Nature Communications, 13(1), 1-8. Summary of the invention

[0020] Technical problem to be solved by the invention

[0021] Indium oxide, one of the crystalline oxide semiconductors, does not contain additive elements, so the film just after sputtering is easily crystallized compared to the oxide material containing indium and additive elements. In order to suppress the crystallization in the film just after sputtering and obtain an amorphous film, hydrogen is used as the sputtering gas. In the case of using hydrogen as the sputtering gas of a large-scale mass production machine, for example, a mixed gas of a rare gas and hydrogen is used. However, as the hydrogen concentration in the mixed gas of the rare gas and hydrogen, it is strongly desired to be below the explosion limit of hydrogen, that is, about 4% based on the volume basis relative to the entire mixed gas.

[0022] In particular, in the case of obtaining an indium oxide thin film, it is difficult to obtain an amorphous thin film in a nearly uniform state on a large-area substrate only by external introduction of a hydrogen concentration of less than 4% by volume during sputtering film formation. As a thin film during sputtering film formation, if an amorphous thin film cannot be obtained, the acid-based processability is reduced, resulting in the inclusion of residues during patterning processing during TFT production. Therefore, in the case of an amorphous thin film in the indium oxide thin film during sputtering film formation, it is difficult to apply the indium oxide thin film to TFT. As such, it is expected that further improvements will be made to the sintered body of an oxide containing indium oxide as the main component, which is the raw material of the sputtering target, so that the oxide thin film provided on the large-area substrate can be uniformly amorphized.

[0023] The object of the present invention is to provide a sputtering target, a method for manufacturing the sputtering target, an oxide thin film using the sputtering target, a thin film transistor including the oxide thin film, and an electronic device including the thin film transistor. The sputtering target comprises an oxide sintered body, and the oxide sintered body is an oxide sintered body that can uniformly form an oxide thin film with excellent TFT processability in a sputtering target having an oxide sintered body containing indium oxide as a main component.

[0024] Solutions for solving the above technical problems [1]

[0026] A sputtering target is a sputtering target comprising an oxide sintered body containing indium oxide as a main component.

[0027] The hydrogen concentration of the oxide sintered body is 5×10 16 atoms / cm 3 above,

[0028] The atomic concentration ratio of the In (indium) element to the O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5,

[0029] The density of the oxide sintered body measured by the Archimedean method was 6.0 g / cm3 above. [2]

[0031] According to the sputtering target described in [1], the hydrogen concentration is 1×10 17 atoms / cm 3 above. [3]

[0033] According to the sputtering target described in [1] or [2], the hydrogen concentration is 1×10 18 atoms / cm 3 above. [4]

[0035] A method for producing a sputtering target is a method for producing the sputtering target described in any one of [1] to [3], comprising:

[0036] A step of obtaining a sintered body raw material containing an indium compound;

[0037] The step of forming the sintered body raw material to obtain a formed body;

[0038] After sintering the compact, the temperature is lowered in an atmosphere containing an inert gas and hydrogen to obtain the oxide sintered body.

[0039] During the temperature reduction process, the temperature is maintained within a range of 800° C. to 1000° C. for at least 3 hours. [5]

[0041] An oxide thin film using the sputtering target described in any one of [1] to [3]. [6]

[0043] A thin film transistor comprises the oxide thin film described in [5]. [7]

[0045] An electronic device comprising the thin film transistor described in [6].

[0046] According to one embodiment of the present invention, there can be provided a sputtering target, a method for manufacturing the sputtering target, an oxide thin film using the sputtering target, a thin film transistor including the oxide thin film, and an electronic device including the thin film transistor. The sputtering target comprises an oxide sintered body, and the oxide sintered body is an oxide sintered body that can uniformly form an oxide thin film with excellent TFT processability in a sputtering target comprising an oxide sintered body containing indium oxide as a main component. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1A This is a perspective view showing the shape of a target according to one embodiment of the present invention.

[0048] Figure 1B This is a perspective view showing the shape of a target according to one embodiment of the present invention.

[0049] Figure 1C This is a perspective view showing the shape of a target according to one embodiment of the present invention.

[0050] Figure 1D This is a perspective view showing the shape of a target according to one embodiment of the present invention.

[0051] Figure 2 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.

[0052] Figure 3 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.

[0053] Figure 4 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.

[0054] Figure 5 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.

[0055] Figure 6 It is a longitudinal cross-sectional view showing a quantum tunnel field effect transistor according to one embodiment of the present invention.

[0056] Figure 7 It is a longitudinal sectional view showing another embodiment of a quantum tunnel field effect transistor.

[0057] Fig. 8A It is a longitudinal cross-sectional view for explaining the manufacturing steps of the quantum tunnel field effect transistor.

[0058] Figure 8B It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.

[0059] Figure 8C It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.

[0060] Fig.8D It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.

[0061] Fig. 8E It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.

[0062] Fig.9A This is a plan view showing a display device using the thin film transistor according to one embodiment of the present invention.

[0063] Fig. 9B1 is a diagram showing a circuit of a pixel portion of a pixel that can be applied to a VA-type liquid crystal display device.

[0064] Fig. 9C This is a diagram showing a circuit of a pixel portion of a display device using an organic EL element.

[0065] Fig.10 This is a diagram showing a circuit of a pixel portion of a solid-state imaging device using a thin film transistor according to one embodiment of the present invention.

[0066] Fig.11A This is an optical microscope image of a semiconductor pattern after the resist in the oxide thin film using the sputtering target according to one embodiment of the present invention has been removed.

[0067] Fig. 11B This is an optical microscope image of a semiconductor pattern after the resist in the oxide thin film using a sputtering target according to one embodiment of the comparative example has been removed. DETAILED DESCRIPTION

[0068] Hereinafter, the embodiments will be described with reference to the accompanying drawings, etc. However, the embodiments can be implemented in a plurality of different schemes, and it is easy for a person skilled in the art to understand that various changes can be made to the embodiments and details without departing from the gist and scope thereof. Therefore, the present invention is not limited to the contents described in the following embodiments for interpretation.

[0069] In the drawings, the size, thickness of the layer, and the region are sometimes exaggerated for clarity. Therefore, the present invention is not limited to the size, thickness of the layer, and the region shown in the drawings. In addition, the drawings schematically show ideal examples, and the present invention is not limited to the shapes and values ​​shown in the drawings.

[0070] Ordinal numbers such as “first”, “second” and “third” used in this specification are added to avoid confusion among components, and components for which no limitation in quantity is described are not limited in quantity.

[0071] In this specification and the like, the term "film" or "thin film" and the term "layer" can be used interchangeably according to circumstances.

[0072] In the sintered body and the oxide thin film in this specification and the like, the term "compound" and the term "crystalline phase" can be used interchangeably according to circumstances.

[0073] In this specification, the "oxide sintered body" may be simply referred to as a "sintered body".

[0074] In this specification, a "sputtering target" may be simply referred to as a "target".

[0075] In this specification, etc., "electrical connection" includes connection via "some substance having an electrical function". Here, "some substance having an electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "some substance having an electrical function" includes electrodes, wiring, switching elements (transistors, etc.), resistors, inductors, capacitors, and other elements with various functions.

[0076] In this specification, etc., the functions of the source or drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current changes during circuit operation. Therefore, in this specification, etc., the terms source or drain can be used interchangeably.

[0077] In the present specification, a numerical range expressed using "to" means a range including the numerical value described before "to" as the lower limit and the numerical value described after "to" as the upper limit.

[0078] The present inventors invented the present invention based on the following findings.

[0079] The present inventors have studied the suppression of residues generated during patterning when manufacturing TFTs (hereinafter, the residues generated during patterning are referred to as patterning residues), making it easier to apply oxide thin films containing indium oxide as a main component to TFTs. In addition, the present inventors have found that by studying the appropriate hydrogen content in the oxide sintered body possessed by the target, the oxide thin film disposed on a large-area substrate can be uniformly amorphized (that is, an oxide thin film with excellent TFT processability can be uniformly formed), and the TFT processability is excellent. In addition, the present inventors have found that in addition to the appropriate hydrogen content in the target, the density of the sintered body and the atomic concentration ratio of the oxygen element to the indium element in the sintered body (O element / In element) are important for uniformly amorphizing the oxide thin film when the oxide thin film containing indium oxide as a main component is disposed on a large-area substrate.

[0080] [Sputtering target]

[0081] The sputtering target of this embodiment uses an oxide sintered body. This sintered body becomes a film raw material when forming a film by sputtering. That is, the sintered body provided by the target of this embodiment is an oxide sintered body containing indium oxide as a main component. The hydrogen content of the sintered body is 5×10 16 atoms / cm 3 The atomic concentration ratio of the In (indium) element to the O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5, and the density of the oxide sintered body measured by the Archimedean method is 6.0 g / cm 3 above.

[0082] In the sintered body possessed by the target of the present embodiment, the sintered body contains indium oxide as the main component and is substantially composed of indium oxide. Relative to the entire sintered body, the sintered body preferably contains more than 99% by mass of indium oxide, and more preferably contains more than 99.9% by mass of indium oxide. In addition, the sintered body contains hydrogen. That is, the sintered body can be substantially composed of only In (indium) element, O (oxygen) element and H (hydrogen) element. Here, "substantially" means that the sintered body of the present embodiment may also contain other components within the range of the effect of the present invention brought about by the combination of the above-mentioned In element and O element. In this case, in the sintered body possessed by the target of the present embodiment, the sintered body may contain elements as impurities.

[0083] Impurities refer to elements that are not intentionally added, and refer to elements mixed in raw materials and manufacturing processes. That is, impurities are inevitable impurities that are inevitably contained. The same applies to the following description. As examples of impurities, for example, at least one element selected from the group consisting of alkali metal elements (elements such as Li (lithium), Na (sodium), K (potassium), Rb (rubidium)), alkaline earth metal elements (elements such as Mg (magnesium), Ca (calcium), Sr (strontium), Ba (barium)), B element (boron element), C element (carbon element), N element (nitrogen element), F element (fluorine element), Si element (silicon element), Zr element (zirconium element), Fe element (iron element), Zn element (zinc element), Sn element (tin element), Al element (aluminum element) and Cl element (chlorine element) can be cited.

[0084] <Atomic concentration ratio (O element / In element)>

[0085] In the sintered body included in the target of the present embodiment, the atomic concentration ratio of the In (indium) element to the O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5.

[0086] When the atomic concentration ratio of oxygen to indium is in the range of 1.3 or more and less than 2.5, the hydrogen concentration contained in the sintered body can be changed by changing the oxygen concentration, so that the oxide thin film provided on a large-area substrate can be uniformly amorphized.

[0087] The atomic concentration ratio of the oxygen element to the indium element is preferably 1.4 or more, more preferably 1.5 or more.

[0088] The atomic concentration ratio of oxygen element to indium element is preferably 2.4 or less, more preferably 2.3 or less.

[0089] The atomic concentration ratio in the sintered body is observed by a scanning electron microscope (SEM: Scanning Electron Microscope), and each element can be quantitatively analyzed by using energy dispersive X-ray analysis (EDX: Energy Dispersive X-ray Spectroscopy). Specifically, first, when the shape of the sputtering target is circular, the square inscribed in the circle is divided into 16 parts with equal area, and the center of each square is observed by SEM under the condition of an acceleration voltage of 10kV in a frame with a magnification of 400 times. When the shape of the sputtering target is a quadrilateral or a cylinder, it is divided into 16 parts with equal area, and the center of each quadrilateral is observed by SEM under the condition of an acceleration voltage of 10kV in a frame with a magnification of 400 times. Then, in each observation area, the X-ray intensity of the In (indium) element and the O (oxygen) element is integrated and converted into atomic concentration by EDX, and the average of each observation point is used as the element concentration ratio of indium to oxygen.

[0090] <Hydrogen concentration>

[0091] The sintered body of the target of this embodiment has a hydrogen content (hydrogen concentration contained in the sintered body) of 5×10 16 atoms / cm 3 If the hydrogen concentration is 5×10 16 atoms / cm 3 The hydrogen concentration in the sintered body is increased, and the oxide thin film provided on a large-area substrate can be uniformly amorphized. From the viewpoint of being able to more easily uniformly amorphize the oxide thin film provided on a large-area substrate, the hydrogen concentration is preferably 7×10 16 atoms / cm 3 More preferably 8×10 16 atoms / cm 3 More preferably, 1×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 above.

[0092] The upper limit of the hydrogen concentration is not particularly limited, but may be, for example, 1×10 20 atoms / cm 3 Below left and right.

[0093] In this specification, the unit of hydrogen concentration [atoms / cm 3 ] is recorded as [atoms·cm -3 ].

[0094] The hydrogen concentration can be quantitatively evaluated using secondary ion mass spectrometry (SIMS). + , sputtering from the surface of the sintered body of the measurement object to a depth of 20μm with an accelerating voltage of 14.5kV. Then, while sputtering with a grating of 100μm square (size of 100μm×100μm), a measurement area of ​​30μm square (size of 30μm×30μm), and a depth of at least 1μm using primary ions, the mass spectrum intensity of the hydrogen concentration is obtained. Furthermore, in order to calculate the absolute value of the hydrogen concentration based on the mass spectrum, hydrogen is injected into the sintered body by controlling the dose through ion implantation to prepare a standard sample (ZnO) with a known hydrogen concentration. By performing SIMS analysis on the standard sample, the mass spectrum intensity of hydrogen is obtained, and the relationship between the absolute value of hydrogen and the mass spectrum intensity is prepared into a standard curve. Finally, the mass spectrum intensity of the sintered body of the measurement object and the standard curve are used to calculate the hydrogen concentration of the measurement object, and it is used as the absolute value of the hydrogen concentration (atoms·cm -3 ).

[0095] In addition, it is known that SIMS analysis is difficult to accurately obtain data near the sample surface and near the lamination interface of a film of different material in principle. Therefore, when analyzing the thickness distribution of hydrogen concentration in a sintered body or an oxide thin film by SIMS, the hydrogen concentration is used as the average value in a region where a substantially constant intensity is obtained without extreme fluctuations within the range where the target film exists.

[0096] The adjustment of the hydrogen concentration contained in the sintered body is not particularly limited. For example, in the sintering process of the sintered body, it can be controlled by the gas atmosphere during the temperature reduction. The gas atmosphere during the temperature reduction is effective, for example, a mixed gas of an inert gas and hydrogen. The method for controlling the hydrogen concentration contained in the sintered body preferably adopts the process described in the method for manufacturing the sputtering target described later.

[0097] <Density>

[0098] The density of the sintered body included in the target of the present embodiment measured by the Archimedean method (hereinafter, sometimes referred to as the density of the sintered body) is 6.0 g / cm 3 If the density of the sintered body is 6.0 g / cm 3 As described above, the generation of target cracks and abnormal discharge during film formation can be suppressed, and a thin film of indium oxide containing hydrogen can be formed in a nearly uniform state. In addition, by making the sintered body high-density, an oxide thin film can be formed under high-output film formation conditions, thereby increasing the film density of the thin film and making it easy to retain hydrogen in the oxide thin film.

[0099] The density of the sintered body is preferably 6.2 g / cm 3 More preferably 6.5 g / cm 3 More preferably, 6.7 g / cm 3 above.

[0100] The upper limit of the density of the sintered body is not particularly limited, but may be 7.2 g / cm 3 Left and right and below.

[0101] The density of the sintered body measured by the Archimedean method is the measured density. In addition, regarding the density of indium oxide, since the density is almost equal to the specific gravity, the value of the specific gravity of the oxide recorded in the Basics of Chemistry Handbook I, edited by the Chemical Society of Japan, revised 2nd edition (Maruzen Co., Ltd.) can be used.

[0102] The shape of the sputtering target is not particularly limited. For example, the sputtering target may be Figure 1A The plate-like shape shown in the reference numeral 1 may also be Figure 1B In the case of a plate-like shape, the planar shape may be Figure 1A The rectangle shown in the figure 1 can also be Figure 1C The oxide sintered body may be formed integrally or as a circle as shown in the figure 1B. Figure 1D As shown, it is a multi-division type in which a plurality of divided oxide sintered bodies (reference numeral 1C) are respectively fixed to a backing plate 3 .

[0103] The sintered body used as the raw material of the target of the present embodiment contains indium oxide as a main component and has (i) a hydrogen concentration of 5×10 16 atoms / cm 3 The above, (ii) the atomic concentration ratio of the In (indium) element to the O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5, and (iii) the density of the oxide sintered body measured by the Archimedean method is 6.0 g / cm 3 All of the above conditions (i) to (iii) can uniformly amorphize an oxide thin film provided on a large-area substrate, thereby suppressing the generation of patterning residues.

[0104] <Other characteristics of sintered body>

[0105] In the sintered body used as the raw material of the target of the present embodiment, the flexural strength of the sintered body is preferably 170 MPa or more, more preferably 180 MPa or more, and even more preferably 200 MPa or more.

[0106] The upper limit of the flexural strength of the sintered body is not particularly limited.

[0107] When the flexural strength of the sintered body is 170 MPa or more, for example, even when a large panel having a large area is produced by a large-scale device, sputtering can be easily performed with cracking of the target suppressed.

[0108] Based on JIS R 1601:2008, prism test pieces were placed on two brackets set at an interval of 30 mm. A load was applied to the pressing piece with the pressing piece abutting against the center portion. The average value of the load (3-point bending strength) at the time of fracture of the 10 test pieces was determined as the flexural strength of the sintered body.

[0109] In the sintered body used as the raw material of the target of the present embodiment, the average crystal grain size of the crystalline phase contained in the sintered body is preferably 10 μm or less, more preferably 5 μm or less, and further preferably 4 μm or less. The lower limit of the average crystal grain size of the sintered body is not particularly limited, and for example, it can be 0.5 μm or more. By making the average crystal grain size of the crystalline phase contained in the sintered body less than 10 μm, the uniformity of the TFT characteristics of the obtained thin film transistor and the reproducibility of the TFT characteristics can be improved. In addition, the average crystal grain size of the crystalline phase contained in the sintered body is measured as the average crystal grain size of the crystalline phase having a pyrolusite structure composed of the In element and the O element.

[0110] The average crystal grain size of the sintered body can be measured using an X-ray microanalyzer (EPMA). Specifically, first, when the shape of the sputtering target is circular, the square inscribed in the circle is divided into 16 parts of equal area, and a sintered body sample is made at the center of each square. When the shape of the sputtering target is a quadrilateral or a cylinder, it is divided into 16 parts of equal area, and a sintered body sample (a total of 16) is made at the center of each quadrilateral. Here, the sintered body sample is a measurement sample. The sintered body sample is made by cutting the sintered body into a size of less than 1 cm square (1 cm × 1 cm in size), and the sintered body sample is embedded in a 1 inch φ epoxy-based room temperature curing resin. Furthermore, the embedded sintered body sample is ground using grinding paper #400, #600, #800, 3μm diamond suspension and 50nm colloidal silica (for final processing) in sequence. Then, the polished surface was magnified 1000 times under the condition of accelerating voltage 10 kV, and the maximum diameter of the crystal grains observed in the 30 μm × 30 μm square frame on the sintered body surface was measured. The maximum diameter of the crystal grains was measured in each of the 16 samples, and the average value of the obtained maximum diameters was taken as the average crystal grain size.

[0111] In the sintered body used as the raw material of the target of the present embodiment, the resistivity of the sintered body is preferably 100 mΩcm or less, more preferably 50 mΩcm or less, and further preferably 30 mΩcm or less. If the resistivity is 100 mΩcm or less, the target is not easily charged during sputtering discharge, the generation of abnormal discharge is suppressed, the plasma state is easily stabilized, and the generation of sparks is suppressed. If the resistivity is large, the target may be charged during sputtering discharge, causing abnormal discharge, or the plasma state may be unstable, causing sparks.

[0112] The resistivity of the sintered body was measured at 10 random locations on the sintered body by a four-probe method (JIS R 1637) using a resistivity meter, and the average value was taken as the resistivity of the sintered body.

[0113] <Method for producing sputtering target>

[0114] An example of a preferred method for producing the target according to the present embodiment will be described.

[0115] Preferably, the method for manufacturing a sputtering target according to the present embodiment includes:

[0116] A step of obtaining a sintered body raw material containing an indium compound (hereinafter sometimes referred to as a sintered body raw material preparation step);

[0117] a step of forming the sintered body raw material to obtain a formed body (hereinafter sometimes referred to as a forming step);

[0118] After sintering the compact, the temperature is lowered in an atmosphere containing an inert gas and hydrogen to obtain the sintered compact (hereinafter sometimes referred to as a sintering step).

[0119] During the temperature reduction process, the temperature is maintained within a range of 800° C. to 1000° C. for at least 3 hours.

[0120] The preferred manufacturing method of the target of this embodiment may also include: at least one of the steps of grinding the sintered body (hereinafter sometimes referred to as the grinding step), cleaning the ground sintered body (hereinafter sometimes referred to as the cleaning step), and joining the sintered body to a backing plate (hereinafter sometimes referred to as the joining step).

[0121] (Sintered body raw material preparation process)

[0122] The sintered body raw material preparation step is a step of preparing a sintered body raw material containing an indium compound. In the sintered body raw material preparation step, first, a raw material powder of an indium compound used as a raw material for a sintered body provided by the sputtering target of the present embodiment is prepared. As the indium compound, for example, at least one of an oxide of indium and a hydroxide of indium can be cited. From the viewpoint of ease of sintering and the viewpoint of suppressing the residual by-products, the indium compound is preferably an oxide of indium (i.e., indium oxide).

[0123] The purity of the indium compound is preferably 2N (99 mass %) or more, more preferably 3N (99.9 mass %) or more, and further preferably 4N (99.99 mass %) or more. By setting the purity of the indium compound to 2N or more, it is easy to ensure the durability of the sintered body. In addition, by setting the purity of the indium compound to 2N or more, for example, when a TFT containing an oxide thin film is used in a liquid crystal display, the possibility of impurities entering the liquid crystal side and causing screen burn-in can be reduced. By using an indium compound with a higher purity, it is easy to obtain an oxide sintered body containing indium oxide as the main component.

[0124] The average particle size of the indium compound is preferably 0.1 μm to 2 μm, more preferably 0.5 μm to 1.5 μm. The average particle size of the indium compound can be measured by a laser diffraction particle size distribution device or the like.

[0125] Next, the prepared raw material powders of the indium compound are mixed and crushed to obtain a raw material mixture. The obtained raw material mixture can be used as a sintered body raw material. A binder can also be added to the raw material powder when the raw material powder is mixed and crushed. The mixing and crushing of the raw material powder can be carried out using a known device such as a ball mill, a bead mill, a jet mill or an ultrasonic device. The conditions for mixing and crushing can be adjusted appropriately. The time for mixing and crushing varies depending on the size of the device and the amount of the raw material mixture processed. The processing time can be adjusted in a manner such that the particle size distribution of the raw material mixture is all in a uniform state close to 1 μm or less. The crushing media (beads) used for the bead mill can include zirconium oxide, aluminum oxide, quartz, silicon nitride, stainless steel, mullite, glass and silicon carbide (SiC).

[0126] The raw material mixture after mixing and crushing can be quickly dried and granulated by spray drying. By granulating the raw material mixture, raw material granulated powder can be obtained. Specifically, a spray dryer is used in the granulation of the raw material mixture after mixing and crushing. The specific drying conditions of the spray dryer are determined by various conditions such as the concentration of the raw material mixture to be dried, the hot air temperature used for drying, the rotation speed and air volume of the spray dryer. When implementing the spray drying method, the optimal conditions can be obtained in advance. The shape of the raw material granulated powder obtained by granulating the raw material mixture is not particularly limited, and is preferably a true spherical shape. The obtained raw material granulated powder can be used as a sintered body raw material.

[0127] In the case where a raw material mixture as a raw material of a sintered body is used without the pre-burning treatment in the pre-burning process described later and the raw material mixture is granulated by a spray drying method, the raw material granulated powder can be prepared by directly using the raw material mixture after mixing and crushing. In the case where a raw material mixture as a raw material of a sintered body is used and the pre-burning treatment in the pre-burning process described later is performed and the raw material mixture is granulated by a spray drying method, the raw material mixture that has been pre-burned can also be crushed again and used as the raw material mixture. In the raw material mixture that has been pre-burned, the particles are bonded to each other, so when a granulation treatment is performed, it is preferred to perform a crushing treatment before the granulation treatment.

[0128] The raw material granulated powder after granulation can be classified to adjust the particle size of the raw material granulated powder. The raw material granulated powder with adjusted particle size can also be used as a sintered body raw material. The classification process can, for example, be a method of sieving the raw material granulated powder that has been subjected to granulation treatment to screen the granulation treatment that belongs to the desired particle size range. The sieve used in this method is preferably a sieve with an opening of a size that the raw material granulated powder of the desired particle size can pass through. The sieve used in this method also preferably uses a first sieve that screens the raw material granulated powder based on the lower limit of the particle size range, and a second sieve that screens the raw material granulated powder based on the upper limit of the particle size range. When the particle size of the raw material granulated powder is controlled within a range of, for example, less than 150 μm, a sieve with an opening of a size that allows raw material granulated powder of less than 150 μm to pass through and prevents raw material granulated powder exceeding 150 μm from passing is used to screen the raw material granulated powder within a range of less than 150 μm.

[0129] Furthermore, when the particle size of the raw material granulated powder is controlled within a range of, for example, 25 μm to 150 μm, first, a sieve (first sieve) having an opening of a size that allows raw material granulated powder smaller than 25 μm to pass through and prevents raw material granulated powder larger than 25 μm from passing through is used to screen the raw material granulated powder having a particle size of 25 μm or larger. Next, the screened raw material granulated powder is screened within a range of 25 μm to 150 μm using a sieve (second sieve) having an opening of a size that allows raw material granulated powder smaller than 150 μm to pass through and prevents raw material granulated powder larger than 150 μm from passing through. The second sieve may be used first, and then the first sieve may be used.

[0130] (Pre-burning process)

[0131] The target manufacturing method of the present embodiment may include a step of pre-firing the sintered body raw material obtained in the raw material preparation step (this step is referred to as a pre-firing step). In the pre-firing step, the sintered body raw material, which is a raw material mixture obtained by mixing and crushing raw material powders, may be pre-firing. In the pre-firing, after obtaining a sintered body raw material of a raw material mixture that is a raw material for a sputtering target, the raw material mixture (i.e., the sintered body raw material) is pre-firing. The pre-firing step is a step provided as needed.

[0132] The density of the obtained sintered body can be easily increased by pre-sintering, so the target manufacturing method of the present embodiment preferably includes a pre-sintering step. On the other hand, from the viewpoint of suppressing cost increase, it is more preferable to increase the density of the sintered body without providing a pre-sintering step.

[0133] In the calcination, the sintered body raw material is preferably heat treated at a temperature range of 500°C to 1200°C for a treatment time of 1 to 100 hours. The calcination is preferably performed at a temperature range of 800°C to 1200°C for a treatment time of 2 to 50 hours.

[0134] By setting the heat treatment conditions to 500° C. or higher and 1 hour or longer, thermal decomposition of the indium compound becomes sufficient.

[0135] On the other hand, by setting the heat treatment conditions to 1200° C. or less and 100 hours or less, the coarsening of particles can be suppressed.

[0136] The calcined product obtained in the calcining step is preferably crushed before the forming step and the firing step described below.

[0137] (Forming process)

[0138] The forming step is a step of forming a sintered body raw material (a sintered body raw material sintered body raw material) by press forming. Through this step, the target is formed into a shape preferred as a target. When the sintering step is provided, the fine powder of the sintered body obtained is granulated and then formed into a desired shape by press forming.

[0139] The average thickness of the molded body is preferably 5.5 mm or more, more preferably 6 mm or more, further preferably 8 mm or more, and particularly preferably 12 mm or more. If the average thickness of the molded body is 5.5 mm or more, the temperature gradient in the thickness direction of the molded body is reduced, and it can be expected that the combination of the surface and deep crystal forms will not change.

[0140] As forming processes that can be used in the forming process, for example, stamping (uniaxial stamping), die forming, casting and injection molding can also be cited. In order to obtain a sintered body (target) with a high sintering density, it is preferred to form it by cold isostatic pressing (CIP: Cold Isostatic Pressing). In addition, it is also possible to set a forming process of two or more stages by forming by cold isostatic pressing (CIP) and hot isostatic pressing (HIP: Hot Isostatic Pressing) after stamping (uniaxial stamping).

[0141] When using a cold isostatic press or a static press, it is preferred to use a surface pressure of 78.5 MPa (800 kgf / cm 2 Converted to SI units) above 392.4MPa (4000kgf / cm 2 The surface pressure is preferably maintained at a pressure of 196.2 MPa or more and 294.3 MPa or less for 2 minutes or less and 30 minutes or less. If it is within the above range, it can be expected that the composition inhomogeneity inside the formed body will be reduced and homogenized. By making the surface pressure above 78.5 MPa, the resistance of the sintered body after sintering can be reduced. By making the surface pressure below 392.4 MPa, it is possible to form without enlarging the device. If the holding time is more than 0.5 minute, it is possible to prevent the resistance after sintering from becoming high. If it is less than 60 minutes, it is possible to prevent excessive time consumption and become uneconomical.

[0142] In the molding process, molding aids such as polyvinyl alcohol, methyl cellulose, polywax, and oleic acid can be used.

[0143] (Sintering process)

[0144] In the sintering step, the molded body obtained in the forming step is sintered to obtain a sintered body. In the sintering step, a commonly used sintering method such as normal pressure sintering, hot pressing sintering, or hot isostatic pressing (HIP) sintering can be used. The obtained sintered body becomes a sputtering target material.

[0145] The sintering temperature is preferably 1200° C. to 1600° C. More preferably, the sintering temperature is 1300° C. to 1500° C.

[0146] The sintering time is preferably from 10 hours to 50 hours, more preferably from 12 hours to 40 hours, and even more preferably from 13 hours to 30 hours.

[0147] If the sintering temperature is 1200°C or higher, the density of the sintered body can be increased, and a density of 6.0 g / cm 3 In addition, if the sintering temperature is 1200°C or more and the sintering time is 10 hours or more, it is easy to fully carry out the sintering, it is easy to fully reduce the resistance of the target, and it is difficult for abnormal discharge to occur. If the sintering temperature is 1600°C or less and the sintering time is 50 hours or less, the increase in the average crystal grain size and the generation of coarse pores caused by significant grain growth can be suppressed, and it is difficult for the sintered body strength to decrease and abnormal discharge to occur.

[0148] In the pressureless sintering method, the compact is sintered in an air atmosphere or an oxygen atmosphere. The oxygen atmosphere preferably has an oxygen concentration of 10% by volume or more and 50% by volume or less. By performing the temperature increase process in an air atmosphere, the density of the sintered compact can be increased.

[0149] In the process of increasing the temperature from 800° C. to the sintering temperature, the temperature increase rate during sintering is preferably 0.1° C. / minute to 2° C. / minute.

[0150] In the sintered body of the present embodiment, the temperature range of 800°C or more is the temperature range in which sintering is most fully performed. If the heating rate in this temperature range is 0.1°C / min or more, excessive grain growth can be suppressed and high density can be achieved. By setting the heating rate to 2°C / min or less, the temperature distribution in the formed body can be suppressed, and the warping or cracking of the sintered body can be suppressed.

[0151] In the process of heating from 800° C. to the sintering temperature, the heating rate is preferably 0.5° C. / min to 2.0° C. / min, more preferably 1.0° C. / min to 1.8° C. / min.

[0152] After sintering, the cooling atmosphere when cooling from the sintering temperature is preferably a mixed gas atmosphere containing an inert gas and hydrogen. Relative to the total of the inert gas and hydrogen, the concentration of hydrogen contained in the mixed gas is preferably in the range of 1 volume % to 5 volume %, more preferably 3 volume % to 5 volume %. The inert gas is not particularly limited, for example, argon is preferably. The cooling during cooling can be left to cool. The cooling rate during cooling is preferably 4°C / minute or less, more preferably 2°C / minute or less, further preferably 1°C / minute or less, further preferably 0.8°C / minute or less, and further preferably 0.5°C / minute or less. If the cooling rate is 4°C / minute or less, cracks are not easily generated during cooling.

[0153] In the process of cooling down in an atmosphere containing hydrogen in an inert gas, as the atmosphere in the sintering furnace, it is preferred to maintain the temperature range of 800°C to 1000°C for at least 3 hours (sometimes the treatment in the cooling process is referred to as the temperature keeping process in the middle of the cooling process). If the temperature is kept at a certain constant temperature in the middle of the cooling process from the sintering temperature, hydrogen can be contained in the target more effectively. Here, maintaining at a certain constant temperature means that in the middle of the cooling process, the temperature in the sintering furnace is maintained at any temperature in the range of 1000°C to 800°C (for example, in the case of maintaining the temperature at 900°C, it is a temperature range of 900°C ± 20°C from 880°C to 920°C). The processing temperature in the temperature keeping process in the middle of the cooling process is more preferably a temperature range of 900°C to 1000°C. The processing time in the temperature keeping process in the middle of the cooling process is more preferably 4 hours or more, more preferably 5 hours or more, and more preferably 7 hours or more. The processing time can be, for example, 10 hours or less. That is, in the process of cooling in an atmosphere containing hydrogen in an inert gas, the temperature is lowered from the sintering temperature, and when the temperature reaches a certain temperature in the temperature range of 800°C to 1000°C (preferably in the temperature range of 900°C to 1000°C), the temperature is maintained near the certain temperature (i.e., the certain temperature in the temperature range of 800°C to 1000°C ± 20°C) for at least 3 hours, and then the temperature is lowered again, thereby easily obtaining a hydrogen concentration of 5×10 16 atoms / cm 3 The above sintered bodies.

[0154] In particular, in the sintering step, by adopting the above-mentioned sintering conditions and temperature reduction conditions, the sintered body that becomes the raw material of the target of this embodiment can meet all of the following conditions: (i) the hydrogen concentration is 5×10 16 atoms / cm 3The above, (ii) the atomic concentration ratio of In (indium) element to O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5, and (iii) the density of the oxide sintered body measured by the Archimedean method is 6.0 g / cm 3 above.

[0155] (Grinding process)

[0156] The grinding step is a step of cutting the sintered body into a shape suitable for installation in a sputtering device. The surface of the sintered body often has at least one of a highly oxidized sintered portion and an uneven surface, and is cut into a specified size.

[0157] In the grinding step, the surface of the sintered body is preferably ground by 0.3 mm or more, more preferably by 0.5 mm or more, and further preferably by 2 mm or more. By grinding the surface of the sintered body by 0.3 mm or more, a variable portion of the crystal structure near the surface can be removed.

[0158] The oxide sintered body is preferably ground, for example, with a surface grinder to produce a raw material having an average surface roughness Ra of 5 μm or less. Furthermore, the sputtering surface of the sputtering target may be mirror-finished to have an average surface roughness Ra of 1000×10 -10 m or less. The mirror finish (grinding) can use known grinding techniques such as mechanical grinding, chemical grinding, mechanochemical grinding (using mechanical grinding and chemical grinding in combination). For example, it can be polished with a fixed abrasive polisher (polishing liquid is water) with #2000 or above, or it can be ground with a free abrasive grinding disc (grinding material is SiC abrasive paste, etc.), and then the grinding material is replaced with diamond abrasive paste to grind. The grinding method is not limited to these methods. The grinding material can be exemplified by a grinding material of #200, #400 or #800.

[0159] (Cleaning process)

[0160] The oxide sintered body after the grinding process is preferably cleaned by a cleaning mechanism such as air blowing and running water cleaning. When removing foreign matter by air blowing, if a vacuum cleaner is used to suck air from the opposite side of the nozzle, the foreign matter can be removed more effectively. In addition, since there are limits to air blowing or running water cleaning, ultrasonic cleaning can be further performed. A method of performing ultrasonic cleaning by multiple oscillations between a frequency of 25kHz or more and 300kHz or less is effective. For example, it is suitable to perform ultrasonic cleaning by multiple oscillations of 12 frequencies every 25kHz between a frequency of 25kHz or more and 300kHz or less.

[0161] (Joining process)

[0162] The bonding step is a step of bonding the sintered body after the processing step to the back plate using a low melting point metal (such as metal indium and metal gallium).

[0163] In terms of maintaining cooling efficiency during sputtering, the bonding rate is preferably 90% or more, more preferably 95% or more, and further preferably 98% or more. The bonding rate referred to herein refers to the area ratio of the surface where the target material and the target support material are bonded via the bonding layer relative to the area of ​​the overlapping surface of the target material and the target support.

[0164] When sputtering film formation is performed using the sputtering target of the present embodiment, an oxide thin film provided on a large-area substrate can be uniformly amorphized, and excellent TFT processability can be obtained.

[0165] [Oxide thin film]

[0166] The oxide thin film of this embodiment is an oxide thin film formed using the sputtering target of this embodiment. The oxide thin film of this embodiment is obtained by forming a film using the sputtering target of this embodiment. The oxide thin film of this embodiment is preferably obtained by a manufacturing method including a step of forming an oxide thin film by sputtering (hereinafter, sometimes referred to as an oxide thin film forming step) and a step of heat-treating the oxide thin film (hereinafter, sometimes referred to as a heat treatment step) using, for example, the sputtering target of this embodiment. According to the oxide thin film of this embodiment, since the film is formed using the target of this embodiment, the processability of the TFT is excellent.

[0167] The oxide thin film of this embodiment is an amorphous oxide thin film after sputtering film formation and before heat treatment (annealing treatment). By performing heat treatment after sputtering film formation, crystallization is improved to become a crystalline oxide thin film. That is, according to the method for manufacturing an oxide thin film of this embodiment, a crystalline oxide thin film can be obtained. In addition, in this embodiment, a crystalline oxide thin film is sometimes referred to as a "crystalline oxide thin film".

[0168] Whether the oxide film is amorphous or crystalline can be confirmed by X-ray diffraction (XRD) measurement. When the oxide film is measured by XRD, if no peak is observed, it can be judged that the oxide film is amorphous, and if a peak is observed, it is judged to be crystalline. In addition, when the oxide film is measured by XRD, if a wide pattern is observed instead of a clear peak, it is judged to be nanocrystalline. On the other hand, when the oxide film is measured by XRD, even if the oxide film can be judged to be amorphous, if patterned residue is confirmed, there is a case of residue being generated. Therefore, even if the oxide film is judged to be amorphous by XRD measurement of the oxide film, it is difficult to judge the degree to which the oxide film is uniformly amorphized.

[0169] In the oxide thin film forming process, a gas that does not substantially contain impurity gas is used. Specifically, in the oxide thin film forming process, one or more gases selected from the group consisting of argon, hydrogen, water vapor and oxygen that do not substantially contain impurity gas are used as sputtering gas. Among them, the sputtering gas is preferably a mixed gas of argon, hydrogen, water vapor and oxygen that does not substantially contain impurity gas, and more preferably a mixed gas of argon, hydrogen and oxygen that does not substantially contain impurity gas. The sputtering gas "substantially does not contain impurity gas" means that, except for the adsorbed water brought in with the insertion of the gas, the leakage of the chamber, and the adsorbed gas and other gases that cannot be removed (inevitable impurity gases), no impurity gas other than argon, hydrogen, water vapor, and oxygen is actively introduced. In this embodiment, as the sputtering gas, for example, any one of a commercially available mixed gas of high-purity argon and high-purity oxygen, a mixed gas of high-purity hydrogen and high-purity argon, and a mixed gas of high-purity hydrogen, high-purity oxygen and high-purity argon can be used. As the sputtering gas, a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon is preferably used. If practicable, it is preferred to remove impurities from the sputtering gas.

[0170] The proportion of the impurity gas in the sputtering gas is preferably 0.1 volume % or less, and more preferably 0.05 volume % or less. If the proportion of the impurity gas is 0.1 volume % or less, crystallization of the oxide thin film proceeds smoothly during annealing after film formation.

[0171] When a mixed gas of high-purity hydrogen, high-purity oxygen and high-purity argon is used, the purity of high-purity argon, high-purity hydrogen and high-purity oxygen is preferably 99 volume % or more, more preferably 99.9 volume % or more, and further preferably 99.99 volume % or more.

[0172] When a mixed gas of high-purity hydrogen, high-purity oxygen and high-purity argon is used as a sputtering gas, the oxygen partial pressure in the mixed gas of argon, hydrogen and oxygen as the sputtering gas is represented by [O2] / ([Ar]+[H2]+[O2]). The oxygen partial pressure is preferably in the range of 0% to 20%. If the oxygen partial pressure is in the above range, it is easy to crystallize and semiconductorize by annealing after film formation. The degree of oxidation, i.e., the degree of crystallization, of the obtained thin film can be adjusted by changing the oxygen partial pressure. The oxygen partial pressure can be appropriately selected as needed.

[0173] When a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon is used as a sputtering gas, the hydrogen partial pressure in the mixed gas of argon, hydrogen, and oxygen as the sputtering gas is represented by [H2] / ([Ar]+[H2]+[O2]). The hydrogen partial pressure is preferably in the range of 0% to 10%, and more preferably in the range of 0% to 5%. The hydrogen content of the semiconductor thin film can be adjusted by changing the hydrogen partial pressure, and the degree of crystallization immediately after film formation can be adjusted. The hydrogen partial pressure can be appropriately selected as needed.

[0174] In the heat treatment step, the heat treatment temperature for crystallizing the formed amorphous thin film is preferably in the range of 200° C. to 500° C., more preferably in the range of 250° C. to 470° C. When the heat treatment temperature is 200° C. or higher, the oxide thin film is easily crystallized.

[0175] If the heat treatment temperature is below 500°C, abnormal crystal growth and grain enlargement can be suppressed. In addition, hydrogen is difficult to escape from the grains and the generation of defect state density is suppressed. Therefore, when used in TFTs, electrical characteristics with good mobility and reliability can be obtained.

[0176] In the heat treatment step, the heat treatment time for crystallizing the formed amorphous thin film is preferably 0.1 to 5 hours, more preferably 0.3 to 3 hours, and even more preferably 0.5 to 2 hours.

[0177] When the heat treatment time is 0.1 hour or longer, crystallization does not occur, and the oxide thin film is easily crystallized.

[0178] When the heat treatment time is 5 hours or less, excellent economic efficiency is achieved.

[0179] The oxide thin film (crystalline oxide thin film) of this embodiment can also be applied to various integrated circuits such as logic circuits, storage circuits and differential amplifier circuits, and these can be applied to electronic devices, etc. In addition, the oxide thin film (crystalline oxide thin film) of this embodiment can be applied as a layer of a part of a solar cell, and a layer of a part of a display device such as a liquid crystal element, an organic electroluminescent element, an inorganic electroluminescent element, a micro organic EL display, a micro LED (Light Emitting Diode) display, and a mini LED display. Furthermore, the oxide thin film (crystalline oxide thin film) of this embodiment can be applied as a layer of a part of a solid-state imaging element, an X-ray sensor, a power semiconductor element, a touch panel, an LSI (Large Scale Integrated circuits), a variable resistance memory, a DRAM (Dynamic Random Access Memory), a ferroelectric memory, a BEOL (Back End of Line) and a microprocessor. The oxide film (crystalline oxide film) of this embodiment can also be suitable as a semiconductor layer of a field effect transistor, a static induction transistor, a quantum tunnel field effect transistor, a Schottky barrier transistor, a Schottky diode, a PN diode and a resistor, and a partial layer thereof.

[0180] [Thin film transistor and electronic device]

[0181] As the thin film transistor of this embodiment, a thin film transistor including the oxide thin film of this embodiment can be mentioned. The oxide thin film of this embodiment is preferably an oxide semiconductor thin film.

[0182] As a channel layer of a thin film transistor, the oxide thin film of this embodiment mode is preferably used.

[0183] When the thin film transistor of this embodiment has the oxide thin film of this embodiment as a channel layer, other element structures in the thin film transistor are not particularly limited, and a known element structure can be adopted.

[0184] The thin film transistor of this embodiment can be suitably used in electronic devices.

[0185] Specifically, the thin film transistor of this embodiment can be suitably used in display devices such as liquid crystal displays and organic EL displays.

[0186] The film thickness of the channel layer in the thin film transistor of this embodiment is usually 10 nm to 300 nm, and preferably 20 nm to 250 nm.

[0187] The channel layer in the thin film transistor of this embodiment is generally used in an N-type region, but can be combined with various P-type semiconductors such as P-type Si-based semiconductors, P-type oxide semiconductors, and P-type organic semiconductors to be used in various semiconductor devices such as PN junction transistors.

[0188] The thin film transistor of this embodiment can also be applied to various integrated circuits such as field effect transistors, logic circuits, storage circuits, and differential amplifier circuits. Furthermore, in addition to field effect transistors, it can also be suitable for electrostatic induction transistors, Schottky barrier transistors, Schottky diodes, and resistors. That is, the thin film transistor of this embodiment can be applied to the uses exemplified in the "Uses of Thin Film Transistors" described later.

[0189] The shape of the thin film transistor of this embodiment is not particularly limited, and is preferably a back channel etch transistor, an etch stop transistor, a top gate transistor, a double gate transistor, etc. In addition, each transistor may have a self-matching (self-aligned) structure.

[0190] Specific examples of thin film transistors are Figure 2 , Figure 3 , Figure 4 and Figure 5 Shown.

[0191] like Figure 2 As shown, the thin film transistor 100 includes a silicon wafer 20 , a gate insulating film 30 , an oxide thin film 40 , a source electrode 50 , a drain electrode 60 , and interlayer insulating films 70 , 70A.

[0192] The silicon wafer 20 is a gate electrode. The gate insulating film 30 is an insulating film that blocks conduction between the gate electrode and the oxide thin film 40 , and is provided on the silicon wafer 20 .

[0193] The oxide thin film 40 is a channel layer, and is provided on the gate insulating film 30. As the oxide thin film 40, the oxide thin film of this embodiment is used.

[0194] The source electrode 50 and the drain electrode 60 are conductive terminals for allowing source current and drain current to flow through the oxide film 40 , and are provided in contact with the vicinity of both ends of the oxide film 40 .

[0195] The interlayer insulating film 70 is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except for the contact portions.

[0196] The interlayer insulating film 70A is an insulating film that blocks conduction except for the contact portion between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is also an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60. The interlayer insulating film 70A is also a channel layer protection layer.

[0197] like Figure 3 As shown, although the structure of the thin film transistor 100A is the same as that of the thin film transistor 100, it is different in that the source electrode 50 and the drain electrode 60 are provided in contact with both the gate insulating film 30 and the oxide thin film 40. It is also different in that the interlayer insulating film 70B is provided integrally in a manner covering the gate insulating film 30, the oxide thin film 40, the source electrode 50, and the drain electrode 60.

[0198] The materials forming the drain electrode 60, the source electrode 50, and the gate electrode are not particularly limited, and any commonly used material can be selected. Figure 2 and Figure 3 In the examples cited above, a silicon wafer is used as a substrate and the silicon wafer also functions as an electrode, but the electrode material is not limited to silicon.

[0199] For example, transparent electrodes such as indium tin oxide (ITO), indium zinc oxide (IZO), ZnO and SnO2, or metal electrodes such as Al, Ag, Cu, Cr, Ni, Mo, Au, Ti and Ta, or metal electrodes or stacked electrodes containing alloys of these metals can be used.

[0200] In addition, Figure 2 , Figure 3 , Figure 4 and Figure 5 In the present invention, a gate electrode can also be formed on a substrate such as glass.

[0201] The material for forming the interlayer insulating films 70, 70A and 70B is not particularly limited, and any commonly used material can be selected. x MN x and MN x O y A compound represented by (wherein M in the formula is a metal element, and x and y are real numbers greater than 0. The same applies to x and y in the compounds exemplified below.) Specifically, the material can be SiO2, SiO x 、SiN x and SiN x O y Furthermore, the material may also include compounds such as Al2O3, Ta2O5, TiO2, MgO, ZrO2, CeO2, K2O, Li2O, Na2O, Rb2O, Sc2O3, Y2O3, HfO2, CaHfO3, PbTiO3, BaTa2O6, SrTiO3, Sm2O3, and AlN. The valence of anions (oxygen anions and nitrogen anions) in these oxide compounds and nitride compounds is not particularly limited as long as it is a real number greater than 0.

[0202] When the thin film transistor of this embodiment is a back channel etch type (bottom gate type), it is preferred to provide a protective film on the drain electrode, the source electrode and the channel layer. By providing a protective film, the durability is easily improved even when the TFT is driven for a long time. In addition, in the case of a top gate type TFT, for example, a gate insulating film is formed on the channel layer.

[0203] When the thin film transistor of this embodiment is a top-gate TFT, for example, an interlayer insulating film is formed on a substrate as a buffer layer, and a gate insulating film is formed on a channel layer. Figure 4 As shown, the thin film transistor 100B has a substrate 21, a buffer layer 22, a channel layer (crystalline oxide thin film) 11, a first low resistance region 11A-1 and a second low resistance region 11A-2 (crystalline oxide thin film), a semiconductor region 11B (crystalline oxide thin film), a gate insulating film 24, a gate electrode 25, an interlayer insulating film 26, a source electrode 27, a drain electrode 28 and a protective film 29. In the thin film transistor 100B, the first low resistance region 11A-1 and the second low resistance region 11A-2 are formed by a dry process such as ion implantation and plasma treatment. In addition, an electrode layer can also be provided between the substrate 21 and the buffer layer 22 as a light blocking layer.

[0204] As another example of the case where the thin film transistor of this embodiment mode is a top-gate TFT, Figure 5 As shown, in the thin film transistor 100C, the interlayer insulating film 26 has a two-layer structure (a first interlayer insulating film 26-1 and a second interlayer insulating film 26-2), and has the same structure as the thin film transistor 100B. In the thin film transistor 100C, the first low resistance region 11A-1 and the second low resistance region 11A-2 are formed by, for example, ion implantation.

[0205] The protective film or insulating film can be formed by, for example, CVD, and a high temperature process may be performed at this time. In addition, the protective film or insulating film often contains impurity gas just after film formation, so it is preferable to perform a heating treatment (annealing treatment). The impurity gas is removed by heating treatment, thereby forming a stable protective film or insulating film, and it is easy to form a TFT element with high durability.

[0206] By using the oxide thin film of this embodiment, the film is less susceptible to the influence of temperature in the CVD process and the influence of the subsequent heat treatment. Therefore, even when a protective film or an insulating film is formed, the stability of TFT characteristics can be improved.

[0207] In the characteristics of the thin film transistor of this embodiment, the on / off ratio is preferably 10 6 above 1012 Below, more preferably 10 7 above 10 11 Below, more preferably 10 8 above 10 10 Below. If the on-off ratio is 10 6 The above is preferred for driving liquid crystal and OLED displays. 12 Below, it is possible to drive an organic EL with a large contrast ratio. 12 Below, the off current can be 10 -11 A or less, when a thin film transistor is used for a transfer transistor or a reset transistor of a CMOS image sensor, it is possible to extend the image retention time or improve the sensitivity.

[0208] The on-off ratio was obtained by setting the value of I d at Vg=-10V as the off current value and the value of I d at Vg=20V as the on current value and determining the ratio [on current value / off current value].

[0209] In the characteristics of the thin film transistor of this embodiment, the threshold voltage (Vth) is preferably -3.0V to 3.0V, more preferably -2.0V to 2.0V, and further preferably -1.0V to 1.0V. If the threshold voltage (Vth) is -3.0V to 3.0V, a Vth correction circuit can be mounted on the TFT to perform correction to Vth = 0V. When the TFT thus obtained is mounted on a panel, the display can be driven without causing uneven brightness and screen burn-in.

[0210] The threshold voltage (Vth) can be calculated from the transfer characteristic graph using the current value Id between the source and the drain = 10 -9 It is defined by the gate voltage Vg under A.

[0211] <Quantum Tunneling Field Effect Transistor>

[0212] The oxide thin film of this embodiment can also be used for a quantum tunnel field effect transistor (FET). In addition, a quantum tunnel field effect transistor is sometimes referred to as a quantum tunnel field effect type transistor.

[0213] exist Figure 6 A schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor (FET) according to one embodiment is shown.

[0214] The quantum tunnel field effect transistor 501 includes a p-type semiconductor layer 503 , an n-type semiconductor layer 507 , a gate insulating film 509 , a gate electrode 511 , a source electrode 513 , and a drain electrode 515 .

[0215] The p-type semiconductor layer 503 , the n-type semiconductor layer 507 , the gate insulating film 509 , and the gate electrode 511 are stacked in this order.

[0216] The source electrode 513 is provided on the p-type semiconductor layer 503 . The drain electrode 515 is provided on the n-type semiconductor layer 507 .

[0217] The p-type semiconductor layer 503 is a p-type Group IV semiconductor layer, and is a p-type silicon layer in this case.

[0218] The n-type semiconductor layer 507 is the n-type oxide thin film in the above-mentioned embodiment. The source electrode 513 and the drain electrode 515 are conductive films.

[0219] Although in Figure 6 Although not shown in the figure, an insulating layer may be formed on the p-type semiconductor layer 503. In this case, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole in a region where the insulating layer is partially opened. Figure 6 Although not shown in the figure, the quantum tunnel field effect transistor 501 may also include an interlayer insulating film covering its upper surface.

[0220] The quantum tunnel field effect transistor 501 is a quantum tunnel field effect transistor (FET) that switches current, and controls the current tunneling through the energy barrier formed by the p-type semiconductor layer 503 and the n-type semiconductor layer 507 by the voltage of the gate electrode 511. In this structure, the band gap of the oxide film constituting the n-type semiconductor layer 507 becomes larger, and the off current can be reduced.

[0221] exist Figure 7 A schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor 501A according to another embodiment is shown.

[0222] The configuration of the quantum tunneling field effect transistor 501A is the same as that of the quantum tunneling field effect transistor 501, but differs in that a silicon oxide layer 505 is formed between the p-type semiconductor layer 503 and the n-type semiconductor layer 507. The presence of the silicon oxide layer can reduce the off current.

[0223] The thickness of the silicon oxide layer 505 is preferably 10 nm or less. By making the thickness of the silicon oxide layer 505 10 nm or less, it is possible to prevent the tunnel current from not flowing, or the energy barrier formed from being difficult to form or the barrier height from changing, thereby preventing the tunnel current from decreasing or changing. The thickness of the silicon oxide layer 505 is preferably 8 nm or less, more preferably 5 nm or less, further preferably 3 nm or less, and further preferably 1 nm or less.

[0224] In the quantum tunneling field effect transistors 501 and 501A, the n-type semiconductor layer 507 is also an n-type oxide semiconductor.

[0225] The oxide thin film constituting the n-type semiconductor layer 507 may also be amorphous. By making the oxide thin film constituting the n-type semiconductor layer 507 amorphous, it can be etched with an organic acid such as oxalic acid, the difference in etching speed with other layers becomes larger, and it will not affect the metal layer such as the wiring, so that etching can be performed well.

[0226] The oxide thin film constituting the n-type semiconductor layer 507 may also be crystalline. By making the oxide thin film constituting the n-type semiconductor layer 507 crystalline, the band gap becomes larger and the off current can be reduced compared to the amorphous case. Since the work function can also be increased, it is easy to control the current that tunnels through the energy barrier formed by the p-type IV group semiconductor material and the n-type semiconductor layer 507.

[0227] The method for manufacturing the quantum tunneling field effect transistor 501 is not particularly limited, and the following method can be exemplified.

[0228] First, if Fig. 8A As shown in FIG. 1 , an insulating film 505A is formed on the p-type semiconductor layer 503 , and a part of the insulating film 505A is opened by etching or the like to form a contact hole 505B.

[0229] Then, if Figure 8B As shown in FIG. 5 , an n-type semiconductor layer 507 is formed on the p-type semiconductor layer 503 and the insulating film 505A. At this time, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole 505B.

[0230] Then, if Figure 8C As shown, a gate insulating film 509 and a gate electrode 511 are sequentially formed on the n-type semiconductor layer 507 .

[0231] Then, if Fig.8D As shown, an interlayer insulating film 519 is provided to cover the insulating film 505A, the n-type semiconductor layer 507 , the gate insulating film 509 , and the gate electrode 511 .

[0232] Then, if Fig. 8E As shown, a contact hole 519A is formed by opening a portion of the insulating film 505A and the interlayer insulating film 519 on the p-type semiconductor layer 503, and a source electrode 513 is provided in the contact hole 519A.

[0233] Furthermore, if Fig. 8E As shown, a contact hole 519B is formed by opening a portion of the gate insulating film 509 and the interlayer insulating film 519 on the n-type semiconductor layer 507, and a drain electrode 515 is formed in the contact hole 519B.

[0234] The quantum tunnel field effect transistor 501 can be manufactured through the above steps.

[0235] After forming the n-type semiconductor layer 507 on the p-type semiconductor layer 503, heat treatment is performed at a temperature of 150°C to 600°C to form the silicon oxide layer 505 between the p-type semiconductor layer 503 and the n-type semiconductor layer 507. By adding this step, the quantum tunnel field effect transistor 501A can be manufactured.

[0236] The thin film transistor of this embodiment is preferably a channel-doped thin film transistor. A channel-doped thin film transistor is a transistor that properly controls the carriers in the channel through n-type doping, rather than oxygen deficiency that is easily changed by external stimuli such as atmosphere and temperature, and can achieve the effect of both high mobility and high reliability.

[0237] <Applications of Thin Film Transistors>

[0238] The thin film transistor of this embodiment can be suitably used in solar cells, display elements (liquid crystal elements, organic electroluminescent elements and inorganic electroluminescent elements, etc.) and power semiconductor elements. The thin film transistor of this embodiment can be suitably used as a transistor for devices using an active matrix method, such as display devices (liquid crystal display, organic EL (Electro Luminescence: electroluminescence) display, micro organic EL display, micro LED (Light Emitting Diode: light emitting diode) display and mini LED display, etc.), solid-state imaging elements and touch panels. The thin film transistor of this embodiment can also be applied to various integrated circuits such as field effect transistors, logic circuits, storage circuits and differential amplifier circuits, and these can be applied to electronic devices, etc. The electronic device of this embodiment preferably includes a thin film transistor. Furthermore, in addition to being suitable for field effect transistors, the thin film transistor of this embodiment can also be suitable for electrostatic induction transistors and Schottky barrier transistors. The thin film transistor of this embodiment can also be suitable as a transistor for sensors such as image sensors, X-ray sensors and biosensors.

[0239] Hereinafter, a case where the thin film transistor of this embodiment is used for a display device and a solid-state imaging element will be described.

[0240] First, refer to Figures 9A to 9C A case where the thin film transistor of this embodiment mode is used in a display device is described.

[0241] Fig.9A It is a top view of the display device of this embodiment. Fig. 9B 2 is a circuit diagram for explaining a circuit of a pixel portion when a liquid crystal element is applied to the pixel portion of the display device of this embodiment. Fig. 9CThis is a circuit diagram for explaining a circuit of a pixel portion in the case where an organic EL element is applied to the pixel portion of the display device of this embodiment.

[0242] The thin film transistor of this embodiment can be used as the transistor configured in the pixel portion. Since the thin film transistor of this embodiment can be easily set to an n-channel type, a part of the driving circuit that can be composed of n-channel transistors is formed on the same substrate as the transistor of the pixel portion. By using the thin film transistor described in this embodiment in the pixel portion or the driving circuit, a display device with high reliability can be provided.

[0243] exist Fig.9A An example of a top view of an active matrix display device is shown. A pixel portion 301, a first scan line driving circuit 302, a second scan line driving circuit 303, and a signal line driving circuit 304 are formed on a substrate 300 of the display device. In the pixel portion 301, a plurality of signal lines are extended from the signal line driving circuit 304, and a plurality of scan lines are extended from the first scan line driving circuit 302 and the second scan line driving circuit 303. Pixels having display elements are arranged in a matrix at the intersection of the scan lines and the signal lines. The substrate 300 of the display device is connected to a timing control circuit (also called a controller, a control IC) via a connection portion such as an FPC (Flexible Printed Circuit).

[0244] exist Fig.9A In the embodiment of the present invention, the first scanning line driving circuit 302, the second scanning line driving circuit 303 and the signal line driving circuit 304 are formed on the same substrate 300 as the pixel portion 301. Therefore, the number of components such as the driving circuit provided outside is reduced, so that cost reduction can be achieved. In addition, when the driving circuit is provided outside the substrate 300, it is necessary to extend the wiring, and the number of connections between the wirings increases. When the driving circuit is provided on the same substrate 300, the number of connections between the wirings can be reduced, thereby achieving improved reliability or improved yield.

[0245] In addition, Fig. 9B An example of a circuit configuration of a pixel is shown. Here, a circuit of a pixel portion that can be applied to a pixel portion of a VA type liquid crystal display device is shown.

[0246] The circuit of the pixel unit can be applied to a structure having multiple pixel electrodes in one pixel. Each pixel electrode is connected to a different transistor, and each transistor is configured to be driven by a different gate signal. Thus, the signal applied to each pixel electrode of the pixel of the multi-domain design can be independently controlled.

[0247] The gate wiring 312 of the transistor 316 and the gate wiring 313 of the transistor 317 are separated so that different gate signals can be provided to the two. On the other hand, the source electrode or the drain electrode 314 functioning as a data line is shared by the transistor 316 and the transistor 317. The thin film transistor of this embodiment can be used for the transistor 316 and the transistor 317. Thus, a liquid crystal display device with high reliability can be provided.

[0248] The first pixel electrode is electrically connected to the transistor 316, and the second pixel electrode is electrically connected to the transistor 317. The first pixel electrode and the second pixel electrode are separated. The shapes of the first pixel electrode and the second pixel electrode are not particularly limited. For example, the first pixel electrode may be V-shaped.

[0249] The gate electrode of transistor 316 is connected to gate wiring 312, and the gate electrode of transistor 317 is connected to gate wiring 313. Different gate signals are supplied to gate wiring 312 and gate wiring 313 to make transistor 316 and transistor 317 operate at different timings, thereby controlling the alignment of liquid crystal.

[0250] Alternatively, a storage capacitor may be formed using the capacitor wiring 310 , a gate insulating film functioning as a dielectric, and a capacitor electrode electrically connected to the first pixel electrode or the second pixel electrode.

[0251] The multi-domain structure includes a first liquid crystal element 318 and a second liquid crystal element 319 in one pixel. The first liquid crystal element 318 is composed of a first pixel electrode, a counter electrode, and a liquid crystal layer therebetween, and the second liquid crystal element 319 is composed of a second pixel electrode, a counter electrode, and a liquid crystal layer therebetween.

[0252] The pixel portion is not limited to Fig. 9B The composition shown. Fig. 9B The pixel portion shown in the figure is further provided with a switch, a resistor, a capacitor, a transistor, a sensor, or a logic circuit.

[0253] exist Fig. 9C Another example of the circuit configuration of a pixel is shown. Here, the configuration of a pixel portion of a display device using an organic EL element is shown.

[0254] Fig. 9C 3 is a diagram showing an example of a circuit of an applicable pixel unit 320. Here, an example of using two n-channel transistors in one pixel is shown. The oxide thin film of this embodiment can be used in the channel formation region of the n-channel transistor. The circuit of the pixel unit can be applied to digital time grayscale driving.

[0255] The thin film transistor of this embodiment can be used as the switching transistor 321 and the driving transistor 322. Thus, a highly reliable organic EL display device can be provided.

[0256] The circuit configuration of the pixel portion is not limited to Fig. 9C The composition shown. Fig. 9C A switch, a resistor, a capacitor, a sensor, a transistor, or a logic circuit is added to the circuit of the pixel portion shown.

[0257] The above is the description of the case where the thin film transistor of this embodiment is used in a display device.

[0258] Next, refer to Fig.10 A case where the thin film transistor of this embodiment is used for a solid-state imaging element will be described.

[0259] CMOS (Complementary Metal Oxide Semiconductor) image sensors are solid-state imaging elements that maintain a potential in a signal charge storage unit and output the potential to a vertical output line via an amplifier transistor. If there is leakage current in the reset transistor and / or transfer transistor included in the CMOS image sensor, the potential of the signal charge storage unit changes due to charging or discharging caused by the leakage current. If the potential of the signal charge storage unit changes, the potential of the amplifier transistor also changes, becoming a value that deviates from the original potential, causing the captured image to deteriorate.

[0260] The effect of operation when the thin film transistor of this embodiment is applied to a reset transistor and a transfer transistor of a CMOS image sensor will be described. The amplifier transistor can be either a thin film transistor or a bulk transistor.

[0261] Fig.10 : This is a diagram showing an example of the pixel structure of a CMOS image sensor. The pixel is composed of a photodiode 3002 as a photoelectric conversion element, a transfer transistor 3004, a reset transistor 3006, an amplifier transistor 3008 and various wirings, and a plurality of pixels are arranged in a matrix to form a sensor. A selection transistor electrically connected to the amplifier transistor 3008 may also be provided. The "OS" marked in the transistor reference numeral represents an oxide semiconductor (Oxide Semiconductor), and "Si" represents silicon, indicating the preferred material when applied to each transistor. The same is true for subsequent drawings.

[0262] The photodiode 3002 is connected to the source side of the transfer transistor 3004, and a signal charge storage unit 3010 (also referred to as FD: Floating diffusion) is formed on the drain side of the transfer transistor 3004. The source of the reset transistor 3006 and the gate of the amplifier transistor 3008 are connected to the signal charge storage unit 3010. As another configuration, the reset power supply line 3110 can also be deleted. For example, there is also a method of connecting the drain of the reset transistor 3006 to the power supply line 3100 or the vertical output line 3120 instead of the reset power supply line 3110.

[0263] In addition, the oxide thin film of this embodiment mode can also be used for the photodiode 3002 , and the same material as the oxide thin film used for the transfer transistor 3004 and the reset transistor 3006 can be used.

[0264] Example

[0265] Hereinafter, the present invention will be described in detail based on Examples. However, the present invention is not limited to the Examples.

[0266] [1] Fabrication of sputtering targets

[0267] (Example 1 to Example 6)

[0268] A sputtering target including an oxide sintered body containing indium oxide as a main component is prepared in the following manner.

[0269] First, indium oxide powder with a purity of 99.99% by mass was prepared as a raw material powder, polyvinyl alcohol, zirconium oxide balls with a diameter of 2 mm and water were added to an alumina pot for crushing, and mixed and crushed for 2 hours using a planetary ball mill. Then, the mixed and crushed mixture was supplied to a spray dryer, and granulated at a rotation speed of 12,000 rpm and a hot air temperature of 150° C. to obtain a raw material granulated powder.

[0270] The raw material granulated powder was passed through a 90-mesh sieve to remove the raw material granulated powder with a particle size exceeding 150 μm, and the particle size of the raw material granulated powder was classified into a range below 150 μm to obtain raw material granulated powder with adjusted particle size. The shape of the obtained raw material granulated powder was a perfect sphere. The raw material granulated powder with adjusted particle size was used as a sintered body raw material. Next, the sintered body raw material was placed in a mold and sieved at 300 kg / cm 2 The stamped body is formed by a pressure of 2600 kg / cm 2 The molded body is obtained by densification through CIP under pressure of.

[0271] The obtained compact was heated to the sintering temperature shown in Table 1 and Table 2 in an air atmosphere by a sintering furnace, and then maintained at the sintering temperature for 20 hours. After sintering, the temperature was cooled from the sintering temperature at a cooling rate of 4°C / min in a mixed gas atmosphere containing argon (Ar) and hydrogen (H2). The concentration of hydrogen in the mixed gas relative to the total (100%) of argon and hydrogen is as shown in Table 1 and Table 2. During the cooling process, the holding time and holding temperature shown in Table 1 and Table 2 were maintained to obtain a sintered compact.

[0272] The obtained sintered body is subjected to surface grinding. After grinding, the surface subjected to surface grinding is used as the sputtering surface, and the surface opposite to the sputtering surface is used as the bonding surface. The bonding surface side of the sintered body is bonded to a backing plate. By bonding to the backing plate, a sputtering target is obtained.

[0273] (Comparative Example 1 to Comparative Example 7)

[0274] A sputtering target was obtained in the same manner as in Example 1 except that the sintering conditions and the temperature drop conditions shown in Tables 3 and 4 were changed to obtain a sintered body.

[0275] [A] Evaluation of sintered body

[0276] [A-1] Measurement of hydrogen concentration

[0277] The hydrogen concentration in the sintered body, which is the raw material of the sputtering target obtained in each of the above-mentioned Examples and Comparative Examples, was quantitatively evaluated by SIMS analysis using a secondary ion mass spectrometer (SIMS analysis device: (manufactured by CAMECA, IMS-6f)).

[0278] First, the surface of the sintered body was plane-polished using abrasive paper #600 and primary ion Cs + , sputtering from the surface of the sintered body of the measured object to a depth of 20μm at an accelerating voltage of 14.5kV. Then, using primary ions to sputter with a grating of 100μm square (size of 100μm×100μm), a measurement area of ​​30μm square (size of 30μm×30μm), and a depth of at least 1μm, the mass spectrum intensity of the hydrogen concentration relative to the film thickness direction is obtained. Furthermore, in order to calculate the absolute value of the hydrogen concentration based on the mass spectrum, hydrogen is injected into the sintered body by controlling the dose through ion implantation to prepare a standard sample (ZnO) with a known hydrogen concentration. For the obtained standard sample, the mass spectrum intensity of hydrogen is obtained by SIMS analysis, and the relationship between the absolute value of hydrogen and the mass spectrum intensity is made into a standard curve.

[0279] Finally, the hydrogen concentration in the film thickness direction of the sintered body to be measured is calculated using the mass spectrum intensity of the sintered body to be measured and the calibration curve.

[0280] The absolute value of the hydrogen concentration (atoms·cm -3 ), the average value of the hydrogen concentration in the region where the change in hydrogen concentration is within 20% and shows a certain intensity at least in the film thickness direction over 20 measurement cycles is taken as the absolute value of the hydrogen concentration.

[0281] In addition, regarding the hydrogen concentration in the sintered body recorded in each embodiment and each comparative example shown in Tables 1 to 4, the square inscribed in the circle of the circular target is divided into 16 parts of equal area, and the hydrogen concentration is evaluated at the center of each square (16 places) using the above-mentioned measurement method, and the average value of the measured values ​​measured at the 16 places is recorded.

[0282] [A-2] Density measurement

[0283] For the raw material of the sputtering target obtained in each of the above-mentioned embodiments and each comparative example, i.e., the oxide sintered body, the sintered body sample for measurement is collected, and the measured density of the sintered body measured by the Archimedean method is measured. Specifically, water is used for measurement at room temperature. In addition, about the density of indium oxide, since the density is almost equal to the specific gravity, the value of the specific gravity of the oxide recorded in the 2nd edition (Maruzen Co., Ltd.) of the Chemical Handbook Basics I, edited by the Chemical Society of Japan, can be used.

[0284] [A-3] Measurement of atomic composition ratio

[0285] The atomic concentration ratio in the raw material, i.e., sintered body, of the sputtering target obtained in each of the above-mentioned embodiments and comparative examples was quantitatively analyzed using a scanning electron microscope (SEM) (manufactured by Hitachi High-Technologies Corporation, SU8200) and an energy dispersive X-ray analyzer (EDX) (manufactured by Hitachi High-Technologies Corporation, S-4800).

[0286] First, a circular sputtering target was divided into 16 squares inscribed in the circle with equal areas, and sintered body samples were prepared at the center (16 locations) of each square.

[0287] Next, each sintered body sample was observed in a frame at a magnification of 400 times under an accelerating voltage of 10 kV using SEM. In the observation area in each sintered body sample (each sintered body sample), the mass spectra of indium and oxygen were integrated using EDX, respectively, and converted into atomic concentrations, and the average of the atomic concentration ratio (O element / In element) in each observation point (16 sintered body samples) was used as the atomic concentration ratio (O element / In element) of indium and oxygen in the sintered body.

[0288] [A-4] Measurement of flexural strength

[0289] The flexural strength of the raw material, i.e., the sintered body, of the sputtering target obtained in each of the above-mentioned examples and comparative examples was measured according to the following procedure. First, 10 prism test pieces with a thickness of 3 mm, a width of 4 mm, and a total length of 36 mm and a rectangular cross section were cut out from the obtained sintered body. Next, the 3-point bending strength was measured using a material testing machine (EZ Graph manufactured by Shimadzu Corporation) based on JIS R 1601:2008, and the average value of the 3-point bending strength measurement values ​​of the 10 test pieces was taken as the flexural strength.

[0290] [A-5] Measurement of average crystal grain size

[0291] The average crystal grain size of the sintered body, which is a raw material of the sputtering target obtained in each of the above Examples and Comparative Examples, was measured using an X-ray microanalyzer (EPMA), namely, JXA-8621MX (manufactured by JEOL Ltd.).

[0292] First, the square inscribed in the circular sputtering target is divided into 16 parts with equal areas, and a sintered body sample is made at the center point 16 of each quadrilateral. The sintered body sample is made by cutting the sintered body into a size of less than 1 cm square (1 cm×1 cm), and the sintered body sample is embedded in a 1 inch φ (1 inch diameter) epoxy-based room temperature curing resin. Furthermore, the embedded sintered body sample is ground using grinding paper #400, #600, #800, 3μm diamond suspension and 50nm colloidal silica (for final processing) in sequence. Then, the ground surface is magnified to 1000 times under the condition of an acceleration voltage of 10kV, and the maximum diameter of the grain (i.e., the crystal phase) observed in the 30μm×30μm square frame on the surface of the sintered body is measured. In the sintered body samples made from 16 places, the maximum diameter of the grain is measured respectively, and the average value of the maximum diameter obtained is taken as the average crystal grain size. The average crystal grain size of the crystal phase included in the sintered body is the average crystal grain size of the crystal phase having a bixbyite structure composed of the In element and the O element.

[0293] [A-6] Measurement of resistivity

[0294] For the average crystal grain size of the raw material of the sputtering target obtained in each of the above-mentioned embodiments and comparative examples, i.e., the sintered body, the resistivity was measured at any 10 locations of the sintered body using a resistivity meter (LORESTA AX MCP-T370 manufactured by Mitsubishi Chemical Corporation) based on the four-probe method (JIS R1637), and the average value was taken as the resistivity of the sintered body.

[0295] [Table 1]

[0296]

[0297] [Table 2]

[0298]

[0299] [Table 3]

[0300]

[0301] [Table 4]

[0302]

[0303] [2] Fabrication of oxide thin films

[0304] (Example 1 to Example 6, Comparative Example 1 to Comparative Example 7)

[0305] Using the sputtering targets obtained in the above-mentioned embodiments and comparative examples, an oxide film (oxide semiconductor film layer) with a thickness of 50 nm is formed by sputtering on a 4-inch silicon wafer (gate electrode) with a thermal oxide film (gate insulating film) with a thickness of 100 nm. In the film formation, a mixed gas of high-purity argon, high-purity oxygen and high-purity hydrogen (specifically, a mixed gas containing (i) high-purity argon, (ii) high-purity oxygen and (iii) a gas containing 5 volume % of high-purity hydrogen mixed in high-purity argon (impurity gas concentration: 0.01 volume %)) is used as the sputtering gas. The film formation conditions are as follows.

[0306] <Film formation conditions>

[0307] Substrate temperature: 25°C

[0308] Ultimate pressure: 4×10 -4 Below Pa

[0309] Atmosphere gas: Ar+O2+H2 (O2 flow ratio 2%_Hydrogen flow ratio 3%)

[0310] Sputtering pressure (total pressure): 0.5Pa

[0311] ·Connection voltage: DC400W

[0312] Magnetic flux density: 600G

[0313] · Distance between S (substrate) and T (target): 70mm

[0314] [B] Evaluation of oxide thin films

[0315] [B-1] Evaluation of patterning residue

[0316] The oxide thin film produced using the sputtering target obtained in each of the above-mentioned embodiments and comparative examples was wet-etched using an organic acid, and the pattern shape after the resist was stripped was observed using an optical microscope to evaluate the patterning residue. In the case where the patterning residue was not generated, it can be judged that the oxide thin film produced using the sputtering target was uniformly amorphized.

[0317] Specifically, a resist is applied to the oxide film prepared as described above, and a pattern of about 20 μm×10 μm is formed by a photolithography process, and etching is performed by an organic acid (manufactured by Kanto Chemical Co., Ltd., ITO-06N) at 25°C. The etching time is reduced by 1.5 times the film thickness of the oxide film. After etching, the photoresist is peeled off to obtain a patterned oxide film. For the patterned oxide film, an optical microscope (manufactured by OLYMPAS, MX51) is used to observe the center and end of a 4-inch silicon wafer substrate to confirm whether residue is generated.

[0318] [Table 5]

[0319] Patterning residue Example 1 No residue Example 2 No residue Example 3 No residue Example 4 No residue Example 5 No residue Example 6 No residue Comparative Example 1 There is residue Comparative Example 2 There is residue Comparative Example 3 There is residue Comparative Example 4 There is residue Comparative Example 5 There is residue Comparative Example 6 There is residue Comparative Example 7 There is residue

[0320] As shown in Table 5, no residue was observed in the oxide thin films of Examples 1 to 6, and a desired pattern was formed. On the other hand, residue was observed in the oxide thin films of Comparative Examples 1 to 7.

[0321] In addition, if Fig.11A As shown in FIG. 1 , using the sputtering target as one embodiment, it was confirmed that no residue was found in the patterned oxide thin film, and a desired pattern was formed. Fig. 11B As shown, when the sputtering target of one embodiment of the comparative example was used, residues were confirmed in the oxide thin film after patterning.

[0322] From the above results, it is understood that the oxide thin film obtained by using the sputtering target of the present embodiment does not generate patterning residue when the oxide thin film is patterned, and thus can be uniformly amorphized, and has excellent TFT processability.

[0323] Description of Reference Numerals

[0324] 1 Oxide sintered body

[0325] 1A oxide sintered body

[0326] 1 B oxide sintered body

[0327] 1 C oxide sintered body

[0328] 3 Back Panel

[0329] 20 Silicon Wafer

[0330] 30Gate insulating film

[0331] 40 oxide film

[0332] 50 Source Electrode

[0333] 60 drain electrode

[0334] 70 interlayer insulation film

[0335] 70A interlayer insulation film

[0336] 70B interlayer insulation film

[0337] 100 Thin Film Transistors

[0338] 100A Thin Film Transistor

[0339] 11Channel layer (crystalline oxide film)

[0340] 11A-1 1st low resistance area

[0341] 11B Semiconductor area

[0342] 11A-2 Second low resistance area

[0343] 21 substrate

[0344] 22 buffer layer

[0345] 24Gate insulating film

[0346] 25 gate electrode

[0347] 26 interlayer insulation film

[0348] 27 Source electrode

[0349] 28 Drain electrode

[0350] 29 Protective film

[0351] 100B Thin Film Transistor

[0352] 100C Thin Film Transistor

[0353] 300 substrates

[0354] 301 Pixel Department

[0355] 302 1st scanning line driving circuit

[0356] 303 second scanning line driving circuit

[0357] 304 signal line driver circuit

[0358] 310 capacitor wiring

[0359] 312 Gate wiring

[0360] 313 Gate wiring

[0361] 314 drain electrode

[0362] 316 transistors

[0363] 317 transistors

[0364] 318 No.1 Liquid Crystal Element

[0365] 319 Second Liquid Crystal Element

[0366] 320 pixels

[0367] 321 Switching Transistor

[0368] 322 driving transistor

[0369] 3002 Photodiode

[0370] 3004 transfer transistor

[0371] 3006 Reset transistor

[0372] 3008 Amplifier Transistor

[0373] 3010 signal charge storage unit

[0374] 3100 Power Cord

[0375] 3110 Reset Power Cord

[0376] 3120 vertical output lines

[0377] 501 Quantum Tunnel Field Effect Transistor

[0378] 501 A Quantum Tunnel Field Effect Transistor

[0379] 503 p-type semiconductor layer

[0380] 505 silicon oxide layer

[0381] 505A Insulation Film

[0382] 505B contact hole

[0383] 507 n-type semiconductor layer

[0384] 509 gate insulation film

[0385] 511 gate electrode

[0386] 513 source electrode

[0387] 515 drain electrode

[0388] 519 interlayer insulation film

[0389] 519A contact hole

[0390] 519B contact hole.

Claims

1. A sputtering target comprising an oxide sintered body containing indium oxide as a main component, characterized in that: The hydrogen concentration of the oxide sintered body is 5×10 16 atoms / cm 3 above, The atomic concentration ratio of the In (indium) element to the O (oxygen) element (O element / In element) is 1.3 or more and less than 2.5, The density of the oxide sintered body measured by the Archimedean method was 6.0 g / cm 3 above.

2. The sputtering target according to claim 1, wherein The hydrogen concentration is 1×10 17 atoms / cm 3 above.

3. The sputtering target according to claim 1 or 2, wherein: The hydrogen concentration is 1×10 18 atoms / cm 3 above.

4. A method for producing a sputtering target, the method being a method for producing the sputtering target according to any one of claims 1 to 3, characterized in that: have: A step of obtaining a sintered body raw material containing an indium compound; The step of forming the sintered body raw material to obtain a formed body; After sintering the compact, the temperature is lowered in an atmosphere containing an inert gas and hydrogen to obtain the oxide sintered body. During the temperature reduction process, the temperature is maintained within a range of 800° C. to 1000° C. for at least 3 hours.

5. An oxide thin film, characterized in that: The sputtering target according to any one of claims 1 to 3 is used.

6. A thin film transistor, characterized in that: Comprising the oxide thin film according to claim 5.

7. An electronic device, characterized in that: A thin film transistor comprising the thin film transistor according to claim 6.