Reflective photomask blank and reflective photomask
By employing a multilayer absorption layer structure with high extinction coefficient and low refractive index in a reflective photomask blank, the phase difference and film thickness are optimized, solving the problems of projection effect and phase shift effect, and improving the transfer resolution of EUV lithography.
Patent Information
- Application Number
- CN202380029334.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-08
AI Technical Summary
During the miniaturization process, existing reflective EUV photomasks suffer from projection effects that degrade transfer performance, and the phase shift effect is not fully utilized, resulting in insufficient resolution.
By combining an absorption control film with a high extinction coefficient and a phase control film with a low refractive index in a reflective photomask blank, a multi-layer absorption layer is formed, controlling the phase difference within the range of 190 degrees to 270 degrees, and the thickness of the absorption layer is less than 60 nm, in order to optimize the phase shift effect.
It improves wafer transfer performance, especially resolution, reduces projection effect, and achieves higher transfer performance.
Smart Images

Figure CN118922779A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a reflective photomask blank and a reflective photomask. Background Art
[0002] In the manufacturing process of semiconductor devices, as semiconductor devices become smaller, the requirements for the miniaturization of photolithography technology also increase accordingly. In photolithography, the minimum resolution size of the transferred pattern depends greatly on the wavelength of the exposure light source. The shorter the wavelength, the smaller the minimum resolution size can be. Therefore, the exposure light source in the manufacturing process of advanced semiconductor devices has been converted from the previous ArF excimer laser with a wavelength of 193nm to EUV (Extreme Ultraviolet) with a wavelength of 13.5nm.
[0003] Since most materials have high light absorption for EUV, the conventional refractive optical system utilizing light transmission cannot be used, so the optical system components of the exposure machine are not lenses but reflectors. The photomask has also changed from the conventional transmission type to a reflective EUV photomask. Since the incident light and reflected light for the EUV photomask cannot be designed on the same axis, the following method is usually used in EUV lithography: the EUV light is incident after the optical axis is tilted 6° from the vertical direction of the EUV photomask, and the reflected light reflected at a negative angle of 6° is irradiated onto the semiconductor substrate. However, since the optical axis is tilted, the EUV light incident on the EUV photomask forms a shadow of the pattern (absorption pattern layer) of the EUV photomask, which may cause a problem of deterioration of the transfer performance, which is called the so-called projection effect (shadow effect). Therefore, reducing the shadow effect and improving the transfer performance have become issues.
[0004] In the existing EUV photomask, a film with a thickness of 60 to 90 nm and tantalum (Ta) as the main component is used as the light absorption layer. When the EUV photomask is used for pattern transfer exposure, line width errors or pattern misalignment may occur on the wafer depending on the line width, orientation, spacing, etc. of the absorption pattern, which deteriorates the transfer quality. In addition, the influence of the projection effect becomes more significant as the line width of the pattern becomes finer.
[0005] To address this problem, a reflective photomask has been proposed that uses a material with a high extinction coefficient k for the absorption layer and forms a thin absorption layer pattern (absorption pattern layer) to reduce the shadowing effect [see, for example, Patent Document 1].
[0006] In addition, with the further miniaturization, the use of a reflective mask blank using a phase shift effect has recently been studied. The phase shift effect is an effect in which the phase of the transmitted light that has passed through the phase shift portion adjacent to the opening is adjusted to be inverse to the phase of the transmitted light that has passed through the opening, thereby reducing the light intensity of the mutually interfering portion of the transmitted light, and as a result, the transfer contrast is improved, thereby improving the resolution of the transferred pattern. Therefore, by also using the phase shift effect in the reflective mask blank, it is expected that the transferability can be further improved.
[0007] For example, in the reflective mask using the phase shift effect described in Patent Document 2, the optimal value of the phase difference is set to 170 to 190 degrees. This value includes the optimal value of the phase difference of 180 degrees of the conventional transmissive phase shift mask.
[0008] However, in the case of a reflective mask, EUV light is incident obliquely, so part of the reflected light passes through the edge of the absorption layer pattern. Since the phase of the reflected light to the edge is offset from that of the reflected light in the center of the pattern, the optimal phase difference of the absorption layer is different from 180 degrees.
[0009] In the reflective mask blank using the phase shift effect described in Patent Document 3, the combination of the film thickness and material composition of the phase shift layer is limited according to the reflectivity and the phase difference for improving the contrast. Therefore, according to the technology described in Patent Document 3, the film thickness of the phase shift layer is reduced to 60 nm or less, and the phase shift effect is obtained while reducing the shadow effect.
[0010] However, Patent Document 3 claims that the film thickness of the phase shift layer is derived from the material and the target reflectivity / phase, and the film thickness is thinner than before, but does not mention the actual transferability. If the phase shift layer is made of a material that absorbs EUV light strongly, such as Ni or Co, even if the film thickness is thinner than before, it may strongly block EUV light incident obliquely and fail to improve the transferability.
[0011] As described above, in the reflective phase shift mask according to the conventional art, the phase shift effect cannot be fully utilized, and the transferability (particularly the resolution) thereof is insufficient.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: International Publication No. 2018 / 159785
[0015] Patent Document 2: Japanese Patent No. 6287099
[0016] Patent Document 3: International Publication No. 2019 / 225737 Summary of the invention
[0017] Problems to be solved by the invention
[0018] The purpose of the present disclosure is to provide a reflective photomask blank and a reflective photomask, wherein an absorption film (absorption layer) is formed by combining an absorption control film for absorbing EUV light and a phase control film for controlling the phase, thereby maximizing the use of the phase shift effect and having high transferability (especially resolution).
[0019] More specifically, the object of the present invention is to provide a reflective photomask and a reflective photomask blank for making the reflective photomask, wherein the absorption film (absorption layer) can be thinned by arranging an absorption control film with a large extinction coefficient k and a phase control film with a small refractive index in the absorption layer, and the transferability can be improved by changing the combination of each layer (each film) of the absorption control film and the phase control film or the film thickness of each layer to have a desired phase difference.
[0020] Means for solving problems
[0021] The present invention is completed to solve the above-mentioned problems. One embodiment of the present invention involves a reflective photomask blank, which is a reflective photomask blank characterized in that it comprises: a substrate, a reflective layer having a multilayer film structure formed on the substrate and reflecting EUV light, a protective layer formed on the reflective layer and protecting the reflective layer, and an absorption layer formed on the protective layer and absorbing EUV light, wherein the absorption layer is composed of a stacked structure of more than two layers with different functions, and the absorption layer has a phase difference in the range of not less than 190 degrees and not more than 270 degrees.
[0022] Furthermore, in the reflective photomask blank according to one embodiment of the present invention, the absorption layer may include an absorption control film.
[0023] In addition, the absorption layer in the reflective photomask blank according to one embodiment of the present invention may include the absorption control film and a phase control film.
[0024] In the reflective photomask blank according to one embodiment of the present invention, the absorption control film may include a material having an extinction coefficient k of 0.041 or more, and the absorption layer may have a thickness of 60 nm or less.
[0025] In addition, the absorption control film in the reflective photomask blank involved in one embodiment of the present invention can be composed of a material containing at least one element of tin (Sn), indium (In), tantalum (Ta), silver (Ag), tellurium (Te), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), palladium (Pd), iridium (Ir), gold (Au) and zinc (Zn).
[0026] In the reflective photomask blank according to one embodiment of the present invention, the absorption layer may include the absorption control film and a phase control film, and the refractive index n of the phase control film with respect to EUV light may be less than 0.93.
[0027] In the reflective photomask blank according to one embodiment of the present invention, the absorption layer may include the absorption control film and a phase control film, and the refractive index n of the phase control film with respect to EUV light may be less than 0.92.
[0028] In addition, the absorption layer in the reflective photomask blank involved in one embodiment of the present invention may have the absorption control film and the phase control film, and the phase control film may be composed of a material containing at least one element of ruthenium (Ru), rhodium (Rh), molybdenum (Mo), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), osmium (Os), iridium (Ir) and rhenium (Re).
[0029] In the reflective photomask blank according to one embodiment of the present invention, the absorption layer may have a phase difference within a range of 210 degrees to 265 degrees.
[0030] In the reflective photomask blank according to one embodiment of the present invention, the absorption layer may have a phase difference within a range of 230 degrees to 260 degrees.
[0031] In addition, a reflective photomask involved in one embodiment of the present invention is a reflective photomask characterized in that it comprises: a substrate, a reflective layer having a multilayer film structure and reflecting EUV light formed on the substrate, a protective layer formed on the reflective layer and protecting the reflective layer, and an absorption pattern layer formed on the protective layer and absorbing EUV light, wherein the absorption pattern layer is composed of a stacked structure of more than two layers with different functions, and the absorption pattern layer has a phase difference in the range of not less than 190 degrees and not more than 270 degrees.
[0032] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may include an absorption control film having a pattern formed therein.
[0033] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may include the absorption control film and a patterned phase control film.
[0034] In the reflective photomask according to one embodiment of the present invention, the absorption control film may include a material having an extinction coefficient k of 0.041 or more, and the absorption pattern layer may have a thickness of 60 nm or less.
[0035] In addition, the absorption control film in the reflective photomask involved in one embodiment of the present invention can be composed of a material containing at least one element of tin (Sn), indium (In), tantalum (Ta), silver (Ag), tellurium (Te), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), palladium (Pd), iridium (Ir), gold (Au) and zinc (Zn).
[0036] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may include the absorption control film and a phase control film having a pattern formed thereon, and the refractive index n of the phase control film with respect to EUV light may be less than 0.93.
[0037] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may include the absorption control film and a phase control film having a pattern formed thereon, and the refractive index n of the phase control film with respect to EUV light may be less than 0.92.
[0038] In addition, the absorption pattern layer in the reflective photomask involved in one embodiment of the present invention may have the absorption control film and a phase control film having a pattern, and the phase control film may be composed of a material containing at least one element of ruthenium (Ru), rhodium (Rh), molybdenum (Mo), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), osmium (Os), iridium (Ir) and rhenium (Re).
[0039] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may have a phase difference within a range of 210 degrees to 265 degrees.
[0040] In the reflective photomask according to one embodiment of the present invention, the absorption pattern layer may have a phase difference within a range of 230 degrees to 260 degrees.
[0041] Effects of the Invention
[0042] According to the reflective photomask blank and the reflective photomask according to one embodiment of the present disclosure, a sufficient phase shift effect can be obtained, and wafer transfer performance (particularly resolution) can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] [ Figure 1 ] is a cross-sectional view showing the structure of a reflective photomask blank according to the present embodiment.
[0044] [ Figure 2 ] is a cross-sectional view showing the structure of the reflective photomask involved in this embodiment.
[0045] [ Figure 3] is a diagram showing the relationship between the phase difference and NILS of a reflective photomask involved in an embodiment of the present invention.
[0046] [ Figure 4 ] is a graph showing the optical constants of various metal materials at the wavelength of EUV light.
[0047] [ Figure 5 ] is a diagram showing the relationship between the phase difference and the film thickness of the reflective photomask involved in an embodiment of the present invention.
[0048] [ Figure 6 ] is a schematic cross-sectional view showing the structure of a reflective photomask involved in an embodiment of the present invention.
[0049] [ Figure 7 ] is a schematic cross-sectional view showing the structure of a reflective photomask blank according to an embodiment of the present invention.
[0050] [ Figure 8 ] is a schematic cross-sectional view showing the manufacturing process of the reflective photomask involved in an embodiment of the present invention.
[0051] [ Fig. 9 ] is a schematic cross-sectional view showing the manufacturing process of the reflective photomask involved in an embodiment of the present invention.
[0052] [ Fig.10 ] is a schematic cross-sectional view showing the manufacturing process of the reflective photomask involved in an embodiment of the present invention.
[0053] [ Fig.11 ] is a schematic cross-sectional view showing the structure of a reflective photomask involved in an embodiment of the present invention.
[0054] [ Fig.12 ] is a schematic cross-sectional view showing the structure of a reflective photomask blank according to a comparative example of the present invention.
[0055] [ Fig.13 ] is a schematic cross-sectional view showing the structure of a reflective photomask involved in a comparative example of the present invention. DETAILED DESCRIPTION
[0056] One embodiment of the present disclosure will be described with reference to the drawings.
[0057] Here, the structure shown in the drawings is schematic, and the relationship between thickness and plane size, the thickness ratio of each layer, etc. are different from the actual situation. In addition, the embodiments shown below illustrate the structure used to concretize the technical idea of the present disclosure. In the technical idea of the present disclosure, the material, shape, structure, etc. of the constituent parts are not limited to the following. The technical idea of the present disclosure can be variously modified within the technical scope specified by the claim items recorded in the claims.
[0058] (Construction of Reflective Photomask Blank and Reflective Photomask)
[0059] Figure 1 1 is a schematic cross-sectional view showing a reflective photomask blank 10 according to an embodiment of the present invention. Figure 1 As shown, a reflective photomask blank 10 according to an embodiment of the present invention comprises: a substrate 1, a reflective layer 2 formed on the substrate 1, a protective layer 3 formed on the reflective layer 2, and an absorption layer 4 formed on the protective layer 3, wherein the absorption layer 4 is composed of at least two layers having different functions. Figure 1 In the example, the absorption layer 4 is constituted of two layers having different functions from each other, one of which is referred to as the absorption layer 4a, and the other layer formed on the absorption layer 4a is referred to as the absorption layer 4b.
[0060] It should be noted that the absorption layers 4a and 4b are either absorption control films or phase control films, and either one of them can be an upper layer or a lower layer. That is, in this embodiment, the absorption layer 4a can be used as an absorption control film and the absorption layer 4b can be used as a phase control film, or the absorption layer 4a can be used as a phase control film and the absorption layer 4b can be used as an absorption control film.
[0061] Furthermore, among the components constituting at least one of the absorption control film and the phase control film, at least one component may have a gradient structure that changes stepwise from the surface layer side toward the substrate 1 side, that is, may have a concentration gradient.
[0062] in addition, Figure 2 2 is a schematic cross-sectional view showing a reflective photomask 20 according to an embodiment of the present invention. Figure 2 The reflective photomask 20 according to the embodiment of the present invention shown in the figure is a reflective photomask 20 which is a reflective photomask 20 according to the embodiment of the present invention. Figure 1 The absorption layer 4 of the reflective photomask blank 10 according to the embodiment of the present invention shown is formed by patterning. Hereinafter, each layer will be described in detail.
[0063] (Substrate)
[0064] The substrate 1 according to the embodiment of the present invention may be, for example, a flat Si substrate or a synthetic quartz substrate. The substrate 1 may be made of low thermal expansion glass to which titanium is added, but any material with a low thermal expansion coefficient may be used and the present invention is not limited thereto.
[0065] Although not shown, a back conductive film may be formed on the surface of the substrate 1 where the reflective layer 2 is not formed. The back conductive film is a film that is fixed by the principle of an electrostatic chuck when the reflective photomask 20 is set on an exposure machine.
[0066] (Reflective layer)
[0067] The reflective layer 2 according to the embodiment of the present invention may be a layer that reflects EUV light (extreme ultraviolet light) as exposure light, and may be a multilayer reflective film formed by combining materials having greatly different refractive indices for EUV light (i.e., an EUV light reflective film having a multilayer film structure). The reflective layer 2 including the multilayer reflective film may be, for example, a layer formed by repeatedly stacking a combination layer such as Mo (molybdenum) and Si (silicon), or Mo (molybdenum) and Be (beryllium) in about 40 cycles.
[0068] (Protective layer)
[0069] The protective layer 3 according to the embodiment of the present invention is a layer that functions as an etching stopper layer to prevent damage to the reflective layer 2 when the absorption pattern 4c is formed by etching. It should be noted that the protective layer 3 may not be formed depending on the material or etching conditions of the reflective layer 2. The protective layer 3 is formed of a material that is resistant to dry etching performed when forming the pattern of the absorption layer 4. For example, the material of the protective layer 3 may be ruthenium (Ru).
[0070] (Absorbent layer)
[0071] like Figure 1 As shown in FIG. 1 , the absorption layer 4 is a layer formed on the protective layer 3 and is a layer for absorbing EUV light as exposure light. In addition, the absorption layer 4 is a layer for forming an absorption pattern 4c as a fine pattern for transfer. That is, by removing a part of the absorption layer 4 of the reflective photomask blank 10, that is, by patterning the absorption layer 4, a Figure 2 The absorption pattern (absorption pattern layer) 4c of the reflective photomask 20 is shown.
[0072] In the absorption pattern 4c, when EUV light is incident and reflected through the pattern opening without passing through the absorption layer 4, the reflected light is affected by the protective layer 3 and the reflective layer 2, and the phase thereof changes from that of the original incident light. On the other hand, when EUV light is incident and (or) reflected through the absorption layer 4, the reflected light is affected by the absorption layer 4 in addition to the protective layer 3 and the reflective layer 2, and the phase thereof changes from that of the original incident light. That is, a desired phase difference is generated based on the film characteristics of the absorption layer 4 between the reflected light generated by the EUV light through the absorption layer 4 and the reflected light generated only through the pattern opening.
[0073] Generally, the phase difference between the absorption layer 4 and the opening portion produced as a result of patterning is uniquely determined as long as the optical constants (refractive index n, extinction coefficient k) and film thickness of each layer of the reflective photomask blank and the reflective photomask, and the wavelength of the light used are determined, and can be calculated by optical theory (for details, see, for example, Applied Physical Engineering Selected Book 3, Yoshida Sadashi "Thin Film", Peifukan, 1990). That is, the "phase difference" in this embodiment refers to the difference between the phase of the reflected light of the absorption layer 4 and the phase of the reflected light (of the opening portion) of the reflective layer 2.
[0074] It should be noted that, in the present embodiment, the values of the refractive index n and the extinction coefficient k used in the calculation of the above-mentioned phase difference are actual measured values using EUV light.
[0075] NILS (Normalized Image Spatial Logarithmic Slope) is obtained by
[0076] NILS=w×dln(I) / dx···Formula (1)
[0077] The obtained contrast value is used as an index of the resolution of the wafer pattern when the wafer pattern is formed using the reflective photomask 20. Here, "w" represents the line width, and "I" represents the intensity of the energy latent image. It should be noted that the larger the NILS value, the higher the resolution of the transferred pattern.
[0078] Figure 3 The relationship between the NILS (Normalized Logarithmic Image Slope) of a wafer pattern when wafer transfer is performed using the reflective photomask 20 , the phase difference of the reflective photomask 20 , and the film thickness of the absorption control film constituting the reflective photomask 20 is shown.
[0079] Figure 3 The graph shows the relationship between the phase difference and the NILS result when exposing a hole pattern of 19 nm on a wafer under the exposure condition of the aperture number NA of 0.33 for a two-layer structure absorption film (absorption layer), with the film thickness of the absorption film (absorption layer) being 43 nm, 44 nm, 45 nm, and 46 nm, respectively. The absorption film is formed by forming an absorption control film composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 (hereinafter, for convenience, also referred to as "absorption control film composed of SnO") as the absorption layer 4a, and forming a phase control film composed of ruthenium (Ru) with a refractive index n of 0.89 as the absorption layer 4b on the absorption control film. It should be noted that the conditions with different phase differences were intentionally prepared by varying the film thickness of SnO and Ru in the range of 0 to 26 nm and 0 to 47 nm, respectively.
[0080] Depend on Figure 3It can be seen that the NILS value is maximum when the phase difference is in the range of approximately 230 degrees to 260 degrees.
[0081] In addition, by Figure 3 It can be seen that when the film thickness is 43 nm and the phase difference is 180 degrees, the NILS value is 2.46.
[0082] Here, when the phase difference is 190 degrees, the NILS is 2.50 at a film thickness of 44 nm, which is 1% or more larger than when the phase difference is 180 degrees at a film thickness of 43 nm.
[0083] In the case where the phase difference is 270 degrees, the NILS is 2.50 at a film thickness of 46 nm, which is 1% or more larger than the case where the phase difference is 180 degrees at a film thickness of 43 nm.
[0084] In the case where the phase difference is 210 degrees, the NILS is 2.64 at a film thickness of 44 nm, which is 7% or more larger than the case where the phase difference is 180 degrees at a film thickness of 43 nm.
[0085] In addition, when the phase difference is 265 degrees, the NILS is 2.64 at a film thickness of 43 nm, which is 7% or more larger than the case where the phase difference is 180 degrees at a film thickness of 43 nm.
[0086] In addition, when the phase difference is 230 degrees, the NILS is 2.74 at a film thickness of 43 nm, which is 11% or more larger than the case where the phase difference is 180 degrees at a film thickness of 43 nm.
[0087] In addition, when the phase difference is 260 degrees, the NILS is 2.74 at a film thickness of 46 nm, which is 11% or more larger than the case where the phase difference is 180 degrees at a film thickness of 43 nm.
[0088] Thus, compared with the case where the phase difference is 180 degrees, if the phase difference is within the range of 190 degrees to 270 degrees, the NILS can be improved by more than 1%, if the phase difference is within the range of 210 degrees to 265 degrees, the NILS can be improved by more than 7%, and if the phase difference is within the range of 230 degrees to 260 degrees, the NILS can be improved by more than 11%.
[0089] It can be seen from this that in order to improve the resolution, the phase difference of the absorption layer 4 is preferably in the range of 190 degrees to 270 degrees, more preferably in the range of 210 degrees to 265 degrees, and most preferably in the range of 230 degrees to 260 degrees.
[0090] Thus, the present inventors have found that the optimum phase difference of the absorption layer in the reflective photomask is a value different from "180 degrees" used in the conventional design concept.
[0091] In EUV lithography, EUV light is incident obliquely and reflected by the reflective layer 2, but due to the projection effect caused by the absorption layer 4 formed with the absorption pattern layer 4c blocking the light path, the transfer performance onto the wafer (semiconductor substrate) may be degraded. By reducing the thickness of the absorption layer 4 that absorbs EUV light, the degradation of the transfer performance can be reduced.
[0092] The film thickness of the absorption layer 4 is preferably 60 nm or less. When the film thickness of the absorption layer 4 is 60 nm or less, since the film thickness is thinner than the conventional Ta-based absorption film (absorption layer), the projection effect can be reduced and the transfer performance can be improved.
[0093] here, Figure 4 This is a diagram showing optical constants of some metal materials with respect to EUV light having a wavelength of 13.5 nm. Figure 4 The horizontal axis represents the refractive index n, and the vertical axis represents the extinction coefficient k. The film thickness of tantalum (Ta), which is the main material of the conventional absorption layer, is 60 to 90 nm. Therefore, if the film thickness of the absorption layer 4 can be set to be less than 60 nm, the transfer performance can be improved compared with the conventional absorption layer (reflective photomask). The film thickness of the absorption layer 4 of the present embodiment is preferably less than 50 nm, more preferably less than 40 nm. It should be noted that in the absorption layer 4 of the present embodiment, there is no particular restriction on its lower limit value, and it is preferably greater than 20 nm, more preferably greater than 25 nm.
[0094] In order to make the absorption control film thinner, it is necessary to use a material having an extinction coefficient k greater than the extinction coefficient k (0.041) of the existing Ta film (a high extinction coefficient material) as the material constituting the absorption control film. In addition, in order to further reduce the thickness of the absorption control film, it is preferred that the extinction coefficient k of the material constituting the absorption control film is 0.05 or more, and more preferably 0.06 or more.
[0095] By using a material having an extinction coefficient k of 0.041 or more as the material constituting the absorption control film, the absorption control film can be sufficiently thinned and the projection effect can be reduced. Specifically, as materials having an extinction coefficient k of 0.06 or more, tin (Sn), indium (In), silver (Ag), tellurium (Te), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), etc. can be listed, as materials having an extinction coefficient k of 0.05 or more, gold (Au), zinc (Zn), etc. can be listed, and as materials having an extinction coefficient k of 0.041 or more, tantalum (Ta), palladium (Pd), iridium (Ir), etc. can be listed. The material constituting the absorption control film is preferably a material containing at least one of these materials (elements). In particular, if the material constituting the absorption control film is an oxide, nitride or oxynitride of Sn, In, or Ta, since these materials have high melting points, it can be expected that the heat resistance of the absorption control film will be further improved and the processability of the absorption control film in the existing etching device will be improved.
[0096] It should be noted that the absorption control film preferably contains 50% by mass or more of the high extinction coefficient material, more preferably 70% by mass or more, and even more preferably 90% by mass or more of the high extinction coefficient material in the overall constituent material. If the content of the high extinction coefficient material is within the above numerical range, the absorption control film can function reliably.
[0097] In this embodiment, the film thickness of the absorption control film is preferably in the range of 1 nm to 30 nm, more preferably in the range of 3 nm to 20 nm, and further preferably in the range of 3 nm to 15 nm. If the film thickness of the absorption control film is within the above numerical range, the absorptivity of EUV light can be easily controlled (adjusted).
[0098] In addition, in the present embodiment, the film thickness of the absorption control film is preferably in the range of 2.5% or more and less than 50% relative to the film thickness of the entire absorption layer 4, more preferably in the range of 10% or more and 40% or less, and further preferably in the range of 10% or more and 30% or less. If the film thickness of the absorption control film is in the above numerical range relative to the film thickness of the entire absorption layer 4, the absorption rate of EUV light can be easily controlled (adjusted).
[0099] Figure 5This is a diagram showing the relationship between the film thickness of the absorption layer 4 and the phase difference when an absorption control film with an extinction coefficient k of 0.07 and a refractive index n of 0.93 is formed in a thickness of less than 1 nm, and a phase control film with an extinction coefficient k of 0.03 and a refractive index n of 0.90, 0.91, 0.92, 0.93, and 0.94 for EUV light is formed thereon by simulation. It should be noted that since the film thickness of the absorption control film is so thin as to be negligible compared with the thickness of the phase control film, the above-mentioned "film thickness of the absorption layer 4" actually refers to the thickness of the phase control film itself.
[0100] like Figure 5 As shown, the smaller the refractive index n of the phase control film constituting the absorption layer 4 is, the thinner the film thickness is for obtaining a desired phase difference.
[0101] Thus, in order to reduce the projection effect, in addition to reducing the film thickness of the absorption control film by increasing the extinction coefficient k of the material constituting the absorption control film, it is also effective to reduce the film thickness of the phase control film by reducing the refractive index n of the material constituting the phase control film.
[0102] like Figure 5 As shown, when the refractive index n of the phase control film constituting the absorption layer 4 is 0.93, the minimum film thickness of the absorption layer 4 (phase control film) for obtaining a phase difference in the range of 230 degrees to 260 degrees is 60nm, which is about the same as the film thickness of the conventional Ta-based absorption film (absorption layer). Therefore, if the refractive index n of the phase control film constituting the absorption layer 4 is less than 0.93, the film thickness of the absorption layer 4 (phase control film) can be made thinner than 60nm, which is preferred. In addition, if the refractive index n of the phase control film constituting the absorption layer 4 is less than 0.92, the minimum film thickness of the absorption layer 4 (phase control film) for obtaining a phase difference in the range of 230 degrees to 260 degrees is 50nm or less, which is more preferred.
[0103] In this embodiment, the film thickness of the phase control film is preferably in the range of 10 nm to 50 nm, more preferably in the range of 15 nm to 40 nm, and further preferably in the range of 20 nm to 30 nm. If the film thickness of the phase control film is within the above numerical range, the phase difference can be easily controlled (adjusted).
[0104] In addition, in the present embodiment, the film thickness of the phase control film is preferably in the range of 50% or more and less than 95% relative to the film thickness of the entire absorption layer 4, more preferably in the range of 60% or more and 85% or less, and further preferably in the range of 70% or more and 80% or less. If the film thickness of the phase control film is in the above numerical range relative to the film thickness of the entire absorption layer 4, the phase difference can be easily controlled (adjusted).
[0105] As described above, the entire absorption layer 4 composed of the phase control film and the absorption control film has a thickness of preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less.
[0106] In the absorption layer 4 composed of the phase control film and the absorption control film, the film thickness of the phase control film is preferably thicker than the film thickness of the absorption control film. For example, the film thickness of the phase control film is preferably 3 times or more, more preferably 5 times or more, and further preferably 8 times or more of the film thickness of the absorption control film.
[0107] By using a material (low refractive index material) having a refractive index n less than 0.93 in the material constituting the phase control film, the phase control film can be sufficiently thinned to reduce the projection effect. Specifically, as materials having a refractive index n less than 0.93, ruthenium (Ru), rhodium (Rh), molybdenum (Mo), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), osmium (Os), iridium (Ir), rhenium (Re), etc. can be listed. The material constituting the phase control film is preferably a material containing at least one of these materials (elements).
[0108] It should be noted that the materials constituting the absorption layer 4, in addition to the above-mentioned materials (i.e., high extinction coefficient materials with an extinction coefficient k greater than 0.041 and low refractive index materials with a refractive index n less than 0.93), for example, by also containing beryllium (Be), calcium (Ca), scandium (Sc), vanadium (V), manganese (Mn), iron (Fe), copper (Cu), germanium (Ge), arsenic (As), strontium (Sr), technetium (Tc), rhodium (Rh), barium (Ba), tungsten (W), rhenium (Re), osmium (Os), gold (Au), etc., it is possible to make a sufficiently amorphous material (a non-crystalline material) that can improve the roughness, in-plane dimensional uniformity, and in-plane uniformity of the transferred image.
[0109] In addition, the materials constituting the absorption layer 4, in addition to the above-mentioned high extinction coefficient materials or low refractive index materials, for example, by also containing chromium (Cr), titanium (Ti), aluminum (Al), silicon (Si), zirconium (Zr), vanadium (V), hafnium (Hf), niobium (Nb), yttrium (Y), lead (Pb), gallium (Ga), etc., it is difficult to react with hydrogen radicals, and a material with better hydrogen radical resistance can be made.
[0110] In addition, the material constituting the absorption layer 4 may contain, in addition to the above-mentioned high extinction coefficient material or low refractive index material, for example, tantalum (Ta), niobium (Nb), chromium (Cr), titanium (Ti), aluminum (Al), vanadium (V), hafnium (Hf), etc. Figure 6As shown, an oxide film 5 having hydrogen radical resistance can be formed to cover the exposed surface of the absorption layer 4. It should be noted that the film thickness of the oxide film 5 is preferably in the range of 1 nm to 5 nm, more preferably in the range of 2 nm to 4 nm, and further preferably in the range of 2.5 nm to 3.5 nm. If the film thickness of the oxide film 5 is within the above numerical range, excellent hydrogen radical resistance is imparted.
[0111] The oxide film 5 is made of a material having a refractive index n close to 1 and an extinction coefficient k close to 0, such as SiO2. If the NILS is higher than that of the conventional Ta-based absorption film, the film thickness may be 10 nm or more. If the film thickness is 10 nm or more, the film can be more resistant to corrosion by the chemical solution during mask cleaning than when the film thickness is thin, and the mask can be used for a long time.
[0112] In addition, regarding the film thickness of the oxide film 5, the film thickness of the oxide film 5 formed on the upper surface of the absorption layer 4 may be thicker than the film thickness of the oxide film 5 formed on the side surface of the absorption layer 4. Since the collision frequency of hydrogen radicals is higher on the upper surface of the absorption layer 4 than on the side surface of the absorption layer 4, if the film thickness of the oxide film 5 formed on the upper surface of the absorption layer 4 is thicker than the film thickness of the oxide film 5 formed on the side surface of the absorption layer 4, the durability of the absorption layer 4 is improved.
[0113] In addition, regarding the film thickness of the oxide film 5, the film thickness of the oxide film 5 formed on the top of the absorption layer 4 may be thinner than the film thickness of the oxide film 5 formed on the side of the absorption layer 4. Since the damage of the absorption layer 4 caused by hydrogen radicals is more likely to affect the transfer performance (especially resolution) on the side of the absorption layer 4 than on the top of the absorption layer 4, when the film thickness of the oxide film 5 formed on the side of the absorption layer 4 is thicker than the film thickness of the oxide film 5 formed on the top of the absorption layer 4, the transfer performance (especially resolution) of the absorption layer 4 is improved.
[0114] In addition, the materials constituting the absorption layer 4, in addition to the above-mentioned high extinction coefficient materials or low refractive index materials, for example, by also containing rhodium (Rh), niobium (Nb), platinum (Pt), titanium (Ti), palladium (Pd), etc., can be made into a material with low reactivity to chemical solutions such as SPM or APM commonly used in mask cleaning and with greater cleaning resistance.
[0115] In addition, the materials constituting the absorption layer 4, in addition to the above-mentioned high extinction coefficient materials or low refractive index materials, for example, by also containing silicon nitride (SiN), tantalum oxide (TaO), etc., can be made into a material that has high absorption of light with a wavelength of 190nm to 260nm and has the ability to improve the contrast of inspection light.
[0116] In addition, the materials constituting the absorption layer 4, in addition to the above-mentioned high extinction coefficient materials or low refractive index materials, for example, by also containing cobalt (Co), ruthenium (Ru), iridium (Ir), gold (Au), palladium (Pd), platinum (Pt), molybdenum (Mo), etc., can make a material with a refractive index n of less than 0.95 for a wavelength of 13.5nm and improved phase shift properties.
[0117] In the above, an example of the effect of the material that can be contained in the absorption layer 4 is described, but the effect of each material is not limited to the above example, and a plurality of effects may be applied.
[0118] It should be noted that, in the overall constituent material of the phase control film, the low refractive index material preferably contains 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. If the content of the low refractive index material is within the above numerical range, the phase control film can function reliably.
[0119] [Example]
[0120] Hereinafter, the present disclosure will be described in more detail through examples, but the present disclosure is not limited to the examples.
[0121] <Example 1>
[0122] like Figure 7 As shown, a synthetic quartz substrate having low thermal expansion is used as the substrate 11. On the substrate 11, 40 laminated films each consisting of a pair of silicon (Si) and molybdenum (Mo) are laminated to form a multilayer reflective film 12. The film thickness of the multilayer reflective film (reflective layer) 12 is set to 280 nm.
[0123] Next, a capping layer (protective layer) 13 was formed on the multilayer reflective film 12 using ruthenium (Ru) to have a film thickness of 3.5 nm. Thus, a reflective portion having the multilayer reflective film 12 and the capping layer 13 was formed on the substrate 11.
[0124] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 is formed on the capping layer 13 in a manner that the film thickness is 9 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 is formed on the absorption control film (lower layer 14a) in a manner that the film thickness is 26 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device), and the result was found to be amorphous. It should be noted that for the above-mentioned absorption control film composed of tin (Sn) and oxygen (O), it is marked as "SnO" in the table for convenience. That is, the composition of the absorption control film composed of tin (Sn) and oxygen (O) in this embodiment is not limited to Sn:O=1:1. The same applies to the following embodiments and comparative examples.
[0125] Next, a back conductive film 15 was formed using chromium nitride (CrN) to a thickness of 100 nm on the side of the substrate 11 where the multilayer reflective film 12 was not formed. A reflective photomask blank 100 was produced.
[0126] A multi-element sputtering device was used to form each film on the substrate 11. The film thickness of each film was controlled by the sputtering time.
[0127] Next, use Figures 8 to 11 The method for manufacturing the reflective photomask 200 is described below. Figure 8 As shown, a positive chemically amplified resist (SEBP9012: manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to the absorption layer 14 of the reflective photomask blank 100 with a thickness of 120 nm by a spin coater and baked at 110° C. for 10 minutes to form a resist film 16 .
[0128] Next, a predetermined pattern is drawn on the resist film 16 using an electron beam drawing machine (JBX3030: manufactured by JEOL Ltd.).
[0129] Then, a pre-baking treatment was performed at 110° C. for 10 minutes, and then a development treatment was performed using a shower developer (SFG3000: manufactured by SigmaMertec). Fig. 9 As shown, a resist pattern 16a is formed.
[0130] Next, using the resist pattern 16a as an etching mask, the phase control film (upper layer 14b) formed of Ru is dry-etched mainly with a fluorine-based gas, and the absorption control film (lower layer 14a) formed of SnO is dry-etched mainly with a chlorine-based gas, thereby patterning the absorption layer 14. Fig.10 As shown, an absorption pattern 14 c is formed on the absorption layer 14 .
[0131] Next, the resist pattern 16a is stripped to produce Fig.11 The reflective photomask 200 according to the present embodiment is shown.
[0132] It should be noted that in this embodiment, the absorption pattern 14 c formed on the absorption layer 14 becomes a hole pattern of 76 nm on the reflective photomask 200 for transfer evaluation.
[0133] The absorption layer 14 of Example 1 formed as described above has a phase difference of 192 degrees at a wavelength of 13.5 nm.
[0134] <Example 2>
[0135] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 13 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 20 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0136] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 2 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0137] The absorption layer 14 of Example 2 formed as described above has a phase difference of 192 degrees at a wavelength of 13.5 nm.
[0138] <Example 3>
[0139] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 8 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 38 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0140] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 3 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0141] The absorption layer 14 of Example 3 formed as described above has a phase difference of 266 degrees at a wavelength of 13.5 nm.
[0142] <Example 4>
[0143] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 1.2 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 44 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0144] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 4 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0145] The absorption layer 14 of Example 4 formed as described above has a phase difference of 266 degrees at a wavelength of 13.5 nm.
[0146] <Example 5>
[0147] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 4 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 39 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0148] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 5 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0149] The absorption layer 14 of Example 5 formed as described above has a phase difference of 248 degrees at a wavelength of 13.5 nm.
[0150] <Example 6>
[0151] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 5 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 39 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0152] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 6 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0153] The absorption layer 14 of Example 6 formed as described above has a phase difference of 248 degrees at a wavelength of 13.5 nm.
[0154] <Example 7>
[0155] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 22 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 22 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0156] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 7 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0157] The absorption layer 14 of Example 7 formed as described above has a phase difference of 210 degrees at a wavelength of 13.5 nm.
[0158] <Example 8>
[0159] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 20 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 27 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0160] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 8 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0161] The absorption layer 14 of Example 8 formed as described above has a phase difference of 263 degrees at a wavelength of 13.5 nm.
[0162] <Example 9>
[0163] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 21 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 19 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0164] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 9 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0165] The absorption layer 14 of Example 9 formed as described above has a phase difference of 230 degrees at a wavelength of 13.5 nm.
[0166] <Example 10>
[0167] An absorption control film (lower layer 14a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 19 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 28 nm. The crystallinity of the absorption layer 14 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0168] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 10 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0169] The absorption layer 14 of Example 10 formed as described above has a phase difference of 260 degrees at a wavelength of 13.5 nm.
[0170] <Example 11>
[0171] An absorption control film (lower layer 14a) composed of tantalum (Ta) with an extinction coefficient k of 0.041 was formed to a film thickness of 4 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 39 nm. The crystallinity of the absorption layer 14 having the tantalum (Ta) film and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0172] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 11 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0173] The absorption layer 14 of Example 11 formed as described above has a phase difference of 246 degrees at a wavelength of 13.5 nm.
[0174] <Example 12>
[0175] An absorption control film (lower layer 14a) composed of niobium (Nb) with an extinction coefficient k of 0.005 was formed to a film thickness of 4 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 39 nm. The crystallinity of the absorption layer 14 having the niobium (Nb) film and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0176] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 12 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0177] The absorption layer 14 of Example 12 formed as described above has a phase difference of 251 degrees at a wavelength of 13.5 nm.
[0178] <Example 13>
[0179] A phase control film (lower layer 14a) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed to a film thickness of 39 nm, and an absorption control film (upper layer 14b) composed of tin (Sn) with an extinction coefficient k of 0.070 and oxygen (O) was formed to a film thickness of 4 nm on the phase control film (lower layer 14a). The crystallinity of the absorption layer 14 having the ruthenium (Ru) film and tin (Sn) and oxygen (O) formed in this way was measured by XRD (X-ray diffraction device), and it was found that it was amorphous.
[0180] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 13 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0181] The absorption layer 14 of Example 13 formed as described above has a phase difference of 248 degrees at a wavelength of 13.5 nm.
[0182] <Example 14>
[0183] An absorption control film (lower layer 14a) composed of indium (In) with an extinction coefficient k of 0.067 and oxygen (O) was formed to a film thickness of 8 nm, and a phase control film (upper layer 14b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 14a) to a film thickness of 36 nm. The crystallinity of the absorption layer 14 having the film composed of indium (In) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0184] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 14 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0185] In addition, the absorption control film composed of indium (In) and oxygen (O) is marked as "InO" in the table for convenience. That is, the composition of the absorption control film composed of indium (In) and oxygen (O) in this embodiment is not limited to In:O=1:1.
[0186] The absorption layer 14 of Example 14 formed as described above has a phase difference of 245 degrees at a wavelength of 13.5 nm.
[0187] <Example 15>
[0188] An absorption control film (lower layer 14a) composed of chromium (Cr) with an extinction coefficient k of 0.039 was formed to a film thickness of 7 nm, and a phase control film (upper layer 14b) composed of niobium (Nb) with a refractive index n of 0.934 was formed on the absorption control film (lower layer 14a) to a film thickness of 62 nm. The crystallinity of the absorption layer 14 having the chromium (Cr) film and the niobium (Nb) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0189] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 15 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0190] The absorption layer 14 of Example 15 formed as described above has a phase difference of 252 degrees at a wavelength of 13.5 nm.
[0191] <Example 16>
[0192] An absorption control film (lower layer 14a) composed of tantalum (Ta) with an extinction coefficient k of 0.041 was formed to a film thickness of 14 nm, and a phase control film (upper layer 14b) composed of niobium (Nb) with a refractive index n of 0.934 was formed on the absorption control film (lower layer 14a) to a film thickness of 53 nm. The crystallinity of the absorption layer 14 having the tantalum (Ta) film and the niobium (Nb) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0193] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 16 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0194] The absorption layer 14 of Example 16 formed as described above has a phase difference of 239 degrees at a wavelength of 13.5 nm.
[0195] <Example 17>
[0196] An absorption control film (lower layer 14a) composed of chromium (Cr) with an extinction coefficient k of 0.039 was formed to a film thickness of 30 nm, and a phase control film (upper layer 14b) composed of molybdenum (Mo) with a refractive index n of 0.923 was formed on the absorption control film (lower layer 14a) to a film thickness of 29 nm. The crystallinity of the absorption layer 14 having the chromium (Cr) film and the molybdenum (Mo) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0197] It should be noted that the reflective photomask blank 100 and the reflective photomask 200 of Example 17 were produced by the same method as that of Example 1 except for the absorption layer 14 .
[0198] The absorption layer 14 of Example 17 formed as described above has a phase difference of 231 degrees at a wavelength of 13.5 nm.
[0199] <Comparative Example 1>
[0200] like Fig.12 As shown, the absorption control film (lower layer 24a) is formed of tantalum nitride (TaN) having an extinction coefficient k of 0.031, and the film thickness is 58nm. In addition, the phase control film (upper layer 24b) is formed of tantalum oxide (TaO) having a refractive index n of 0.95, and the film thickness is 2nm. The crystallinity of the absorption layer 24 having the tantalum nitride (TaN) film and the tantalum oxide (TaO) film formed in this way was measured by XRD (X-ray diffraction device), and the result was found to be amorphous. Here, this comparative example assumes a conventional reflective photomask with an existing film having tantalum (Ta) as the main component.
[0201] It should be noted that, except for the formation of the absorption layer 24, the same method as in Example 1 was used to prepare the Fig.12 and Fig.13 The reflective photomask blank 101 of Comparative Example 1 and the reflective photomask 201 including the absorption pattern 24 c are shown.
[0202] The absorption layer 24 of Comparative Example 1 formed as described above has a phase difference of 160 degrees at a wavelength of 13.5 nm.
[0203] <Comparative Example 2>
[0204] An absorption control film (lower layer 24a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 11 nm, and a phase control film (upper layer 24b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 24a) to a film thickness of 24 nm. The crystallinity of the absorption layer 24 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0205] It should be noted that the reflective photomask blank 101 and the reflective photomask 201 of Comparative Example 2 were produced by the same method as in Example 1 except for the absorption layer 24 .
[0206] The absorption layer 24 of Comparative Example 2 formed as described above has a phase difference of 180 degrees at a wavelength of 13.5 nm.
[0207] <Comparative Example 3>
[0208] An absorption control film (lower layer 24a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 7 nm, and a phase control film (upper layer 24b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 24a) to a film thickness of 40 nm. The crystallinity of the absorption layer 24 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0209] It should be noted that the reflective photomask blank 101 and the reflective photomask 201 of Comparative Example 3 were produced by the same method as in Example 1 except for the absorption layer 24 .
[0210] The absorption layer 24 of Comparative Example 3 formed as described above has a phase difference of 284 degrees at a wavelength of 13.5 nm.
[0211] <Comparative Example 4>
[0212] An absorption control film (lower layer 24a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 15 nm, and a phase control film (upper layer 24b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 24a) to a film thickness of 22 nm. The crystallinity of the absorption layer 24 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0213] It should be noted that the reflective photomask blank 101 and the reflective photomask 201 of Comparative Example 4 were produced by the same method as in Example 1 except for the absorption layer 24 .
[0214] The absorption layer 24 of Comparative Example 4 formed as described above has a phase difference of 188 degrees at a wavelength of 13.5 nm.
[0215] <Comparative Example 5>
[0216] An absorption control film (lower layer 24a) composed of tin (Sn) and oxygen (O) with an extinction coefficient k of 0.070 was formed to a film thickness of 1 nm, and a phase control film (upper layer 24b) composed of ruthenium (Ru) with a refractive index n of 0.89 was formed on the absorption control film (lower layer 24a) to a film thickness of 30 nm. The crystallinity of the absorption layer 24 having the film composed of tin (Sn) and oxygen (O) and the ruthenium (Ru) film formed in this way was measured by XRD (X-ray diffraction device) and was found to be amorphous.
[0217] It should be noted that the reflective photomask blank 101 and the reflective photomask 201 of Comparative Example 5 were produced by the same method as in Example 1 except for the absorption layer 24 .
[0218] The absorption layer 24 of Comparative Example 5 formed as described above has a phase difference of 188 degrees at a wavelength of 13.5 nm.
[0219] <Evaluation>
[0220] The transfer performance of the reflective photomasks obtained in Examples 1 to 17 and Comparative Examples 1 to 5 was evaluated by the following method. The transfer performance was confirmed by wafer exposure evaluation. In addition, the resolution was evaluated by NILS (Normalized Image Log-Slope).
[0221] Using an EUV exposure device (NXE3300B: manufactured by ASML), the absorption pattern of the reflective photomask produced in each embodiment and comparative example was transferred and exposed on a semiconductor wafer coated with an EUV positive chemical amplification resist. At this time, the exposure amount was adjusted so that the hole pattern was transferred according to the designed 19nm. Then, the transferred resist pattern was observed using an electron beam size measuring instrument and the line width was measured to confirm the resolution, which was evaluated using the following four levels of "◎", "○", "△", and "×".
[0222] <Evaluation Criteria>
[0223] ◎: When the NILS value is 2.60 or more
[0224] ○: NILS value is 2.50 or more and less than 2.60
[0225] △: When the NILS value is 2.47 or more and less than 2.50
[0226] ×: NILS value is less than 2.47
[0227] The above evaluation results are shown in Table 1.
[0228] In addition, regarding the NILS value, if it is evaluated as "△" or more, there is no problem in the transfer performance, and it is regarded as passing.
[0229] [Table 1]
[0230]
[0231] Table 1 shows the evaluation results of Examples 1 to 17 and Comparative Examples 1 to 5.
[0232] Comparative Example 1 having a conventional 60 nm thick tantalum (Ta) absorption layer has a phase difference of 160 degrees and a NILS of 2.37. It is found that when the phase difference of the absorption pattern layer is 190 degrees or more and 270 degrees or less as in Examples 1 to 17, the NILS is larger than that in Comparative Example 1 and the resolution is improved.
[0233] Below, using Table 1 and Figure 3 , Figure 5 The figures shown in the figure explain in detail the results of NILS comparison of each example and each comparative example.
[0234] When comparing Example 1, Example 3 and Example 5, when the phase difference is 192 degrees, 266 degrees and 248 degrees respectively, the NILS is 2.61, 2.60 and 2.81 respectively, and all are evaluated as "◎". In Comparative Examples 2 and 3, when the phase difference is 180 degrees and 284 degrees respectively, the NILS is 2.46 and 2.34 respectively, and all are evaluated as "×".
[0235] It can be seen from this that sufficient resolution is achieved when the phase difference is between 190 degrees and 270 degrees. That is, the range of the appropriate phase difference of the absorption layer in the reflective photomask is different from the "180 degrees" used in the previous design concept, and can be said to be "within the range of 190 degrees and 270 degrees".
[0236] When comparing Example 1, Example 3, and Example 5, when the phase differences were 192 degrees, 266 degrees, and 248 degrees, respectively, the NILS were 2.61, 2.60, and 2.81, respectively, and all were evaluated as "◎".
[0237] When comparing Example 7, Example 8, Example 9 and Example 10, the phase differences are 210 degrees, 263 degrees, 230 degrees and 260 degrees respectively. Here, NILS in Example 7, Example 8, Example 9 and Example 10 are 2.65, 2.70, 2.75 and 2.72 respectively, and all are evaluated as "◎".
[0238] In addition, if Figure 3 As shown, compared with the case where the phase difference is 180 degrees, if the phase difference is in the range of 190 degrees to 270 degrees, the NILS can be improved by more than 1%, if the phase difference is in the range of 210 degrees to 265 degrees, the NILS can be improved by more than 7%, and if the phase difference is in the range of 230 degrees to 260 degrees, the NILS can be improved by more than 11%.
[0239] It can be seen from this that in order to improve the resolution, the phase difference of the absorption layer is preferably in the range of 190 degrees to 270 degrees, more preferably in the range of 210 degrees to 265 degrees, and most preferably in the range of 230 degrees to 260 degrees.
[0240] When comparing Example 5, Example 11, and Example 12, the film thickness of the absorption control film is the same as the film thickness of the Ru film as the phase control film. It should be noted that the materials used in the absorption control films of Example 5, Example 11, and Example 12 are SnO (extinction coefficient k is 0.070), Ta (extinction coefficient k is 0.041), and Nb (extinction coefficient k is 0.005), respectively. Here, NILS is 2.81, 2.75, and 2.59 in the case of Example 5, Example 11, and Example 12, respectively.
[0241] Comparing Example 5 with Example 13, the film thickness of SnO as the absorption control film and the film thickness of Ru film as the phase control film are the same, but the positions of the layers are swapped. Here, the phase difference and NILS are all equal, 248 degrees and 2.81 respectively.
[0242] It can be seen from this that when the absorption layer has a two-layer structure, even if the upper and lower layers are swapped, the phase difference and NILS are all equal.
[0243] When comparing Example 5 and Example 14, the materials used in the absorption control films of Example 5 and Example 14 are SnO (extinction coefficient k is 0.070) and InO (extinction coefficient k is 0.067), respectively, and the extinction coefficient of each material is greater than 0.041. Here, NILS is 2.81 and 2.82 in the case of Example 5 and Example 14, respectively.
[0244] This shows that when a material having a large extinction coefficient k, such as tin oxide (Sn) or indium oxide (In), is used in the absorption control film, the resolution is improved.
[0245] When comparing Comparative Example 4 and Comparative Example 5, the phase difference is 188 degrees. Here, NILS is 2.44 and 1.34 in Comparative Example 4 and Comparative Example 5, respectively. The NILS in both cases is evaluated as "×".
[0246] It should be noted that the reflective photomask blank and the reflective photomask disclosed herein are not limited to the above-described embodiments and examples, and various modifications may be made within a scope not impairing the characteristics of the invention.
[0247] Industrial Applicability
[0248] The reflective photomask blank and the reflective photomask according to the present invention can be suitably used for forming a fine pattern by EUV exposure in the manufacturing process of semiconductor integrated circuits and the like.
[0249] Explanation of symbols
[0250] 1...Substrate
[0251] 2…Reflective layer
[0252] 3…Protective layer
[0253] 4…Absorption layer
[0254] 4a…Absorbent layer (lower layer)
[0255] 4b…Absorbent layer (upper layer)
[0256] 4c…Absorption pattern
[0257] 5…Oxide coating
[0258] 5a…Oxide coating pattern
[0259] 10…Reflective photomask blank
[0260] 20…Reflective photomask
[0261] 11…Substrate
[0262] 12…Reflection layer
[0263] 13…Protective layer
[0264] 14…Absorption layer
[0265] 14a…absorption layer (lower layer)
[0266] 14b…absorption layer (upper layer)
[0267] 14c…Absorption pattern
[0268] 15…Back conductive film
[0269] 16…Resist film
[0270] 16a…Resist pattern
[0271] 100…Reflective photomask blank
[0272] 200…Reflective photomask
[0273] 24…Absorption layer
[0274] 24a…absorption layer (lower layer)
[0275] 24b…absorption layer (upper layer)
[0276] 24c…Absorption pattern
[0277] 101…Reflective photomask blank
[0278] 201…Reflective photomask
Claims
1. A reflective photomask blank, characterized in that: have: substrate, a reflective layer having a multi-layer film structure and reflecting EUV light formed on the substrate, a protective layer formed on the reflective layer and protecting the reflective layer, and an absorption layer formed on the protective layer and absorbing EUV light, The absorption layer is composed of a laminated structure of two or more layers with different functions. The absorption layer has a phase difference in the range of 190 degrees to 270 degrees.
2. The reflective photomask blank according to claim 1, wherein: The absorption layer has at least an absorption control film.
3. The reflective photomask blank according to claim 2, wherein: The absorption layer has the absorption control film and a phase control film.
4. The reflective photomask blank according to claim 2 or claim 3, characterized in that: The absorption control film contains a material with an extinction coefficient k of 0.041 or more, The absorption layer has a thickness of 60 nm or less.
5. The reflective photomask blank according to any one of claims 2 to 4, characterized in that: The absorption control film is composed of a material containing at least one element selected from the group consisting of tin (Sn), indium (In), tantalum (Ta), silver (Ag), tellurium (Te), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), palladium (Pd), iridium (Ir), gold (Au) and zinc (Zn).
6. The reflective photomask blank according to any one of claims 2 to 5, characterized in that: The absorption layer has the absorption control film and the phase control film, The refractive index n of the phase control film with respect to EUV light is less than 0.
93.
7. The reflective photomask blank according to any one of claims 2 to 5, characterized in that: The absorption layer has the absorption control film and the phase control film, The refractive index n of the phase control film with respect to EUV light is less than 0.
92.
8. The reflective photomask blank according to any one of claims 2 to 7, characterized in that: The absorption layer has the absorption control film and the phase control film, The phase control film is composed of a material containing at least one element selected from the group consisting of ruthenium (Ru), rhodium (Rh), molybdenum (Mo), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), osmium (Os), iridium (Ir) and rhenium (Re).
9. The reflective photomask blank according to any one of claims 1 to 8, characterized in that: The absorption layer has a phase difference in the range of not less than 210 degrees and not more than 265 degrees.
10. The reflective photomask blank according to any one of claims 1 to 8, characterized in that: The absorption layer has a phase difference in the range of 230 degrees to 260 degrees.
11. A reflective photomask, characterized in that: have: substrate, a reflective layer having a multi-layer film structure and reflecting EUV light formed on the substrate, a protective layer formed on the reflective layer and protecting the reflective layer, and an absorption pattern layer formed on the protective layer and absorbing EUV light, The absorption pattern layer is composed of a stacked structure of two or more layers with different functions. The absorption pattern layer has a phase difference in the range of 190 degrees to 270 degrees.
12. The reflective photomask according to claim 11, wherein: The absorption pattern layer at least has an absorption control film having a pattern formed therein.
13. The reflective photomask according to claim 12, wherein: The absorption pattern layer includes the absorption control film and a phase control film having a pattern formed therein.
14. The reflective photomask according to claim 12 or claim 13, characterized in that: The absorption control film contains a material with an extinction coefficient k of 0.041 or more, The absorption pattern layer has a film thickness of 60 nm or less.
15. The reflective photomask according to any one of claims 12 to 14, wherein: The absorption control film is composed of a material containing at least one element selected from the group consisting of tin (Sn), indium (In), tantalum (Ta), silver (Ag), tellurium (Te), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), palladium (Pd), iridium (Ir), gold (Au) and zinc (Zn).
16. The reflective photomask according to any one of claims 12 to 15, characterized in that: The absorption pattern layer has the absorption control film and a phase control film having a pattern formed thereon, The refractive index n of the phase control film with respect to EUV light is less than 0.
93.
17. The reflective photomask according to any one of claims 12 to 15, characterized in that: The absorption pattern layer has the absorption control film and a phase control film having a pattern formed thereon, The refractive index n of the phase control film with respect to EUV light is less than 0.
92.
18. The reflective photomask according to any one of claims 12 to 17, wherein: The absorption pattern layer has the absorption control film and a phase control film having a pattern formed thereon, The phase control film is composed of a material containing at least one element selected from the group consisting of ruthenium (Ru), rhodium (Rh), molybdenum (Mo), palladium (Pd), silver (Ag), platinum (Pt), gold (Au), osmium (Os), iridium (Ir) and rhenium (Re).
19. The reflective photomask according to any one of claims 11 to 18, wherein: The absorption pattern layer has a phase difference in the range of not less than 210 degrees and not more than 265 degrees.