Positive photosensitive resin composition, cured film, and semiconductor device

By using biphenyl phenolic resin, crosslinking agent and photosensitive agent in the positive photosensitive resin composition, the problem of insufficient cured film strength under low temperature conditions is solved, and a resin film with high tensile fracture strength is realized, and the semiconductor is improved Reliability of the device and cured film properties.

CN118922781APending Publication Date: 2024-11-08SUMITOMO BAKELITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029949.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to improve the reliability of electronic devices and the mechanical strength of the cured film under low temperature conditions. Especially when the thermal damage of semiconductor chips is reduced, the heating temperature of traditional thermosetting resin compositions is high, which affects the performance of the cured film. .

Method used

Using a positive photosensitive resin composition containing a biphenyl phenolic resin, a specific crosslinking agent and a photosensitive agent, a resin film with high tensile breaking strength was obtained by curing at 180°C, and used for the rewiring layer of a semiconductor device, which improves the Low temperature curability and mechanical properties.

Benefits of technology

The cured film with excellent mechanical strength obtained under low temperature conditions is achieved, which improves the reliability of the semiconductor device and the performance of the cured film, and meets the dual demands of low temperature curing and high mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005057185630000031
    Figure BDA0005057185630000031
  • Figure BDA0005057185630000041
    Figure BDA0005057185630000041
  • Figure BDA0005057185630000081
    Figure BDA0005057185630000081
Patent Text Reader

Abstract

A positive photosensitive resin composition, which can be used in a rewiring layer of a semiconductor device, contains (A) a phenolic resin having a diphenol structure, (B) a crosslinking agent, and (C) a photosensitizer, and the tensile breaking strength of a cured product obtained by curing the positive photosensitive resin composition at 180 DEG C is 100 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive photosensitive resin composition and a cured film thereof, and a semiconductor device having the cured film as an insulating layer. Background Art

[0002] In the electrical / electronic field, a photosensitive resin composition containing a thermosetting resin is sometimes used to form a cured film such as an insulating layer. Therefore, a photosensitive resin composition containing a thermosetting resin has been studied so far. It is known that an insulating film in a rewiring layer and an insulating film in a portion other than the rewiring layer are formed using a photosensitive resin composition containing a thermosetting resin.

[0003] As an example, a photosensitive resin composition containing an alkaline aqueous solution soluble resin, a crosslinking agent, a photopolymerization initiator, and an epoxy resin (thermosetting resin) represented by a specific general formula is described in Patent Document 1. Patent Document 1 describes that the photosensitive resin composition has good photosensitivity. In addition, Patent Document 1 describes that a film formed from the photosensitive resin composition is excellent in terms of bendability, adhesion, pencil hardness, solvent resistance, acid resistance, heat resistance, gold plating resistance, and the like.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-80871 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] As electronic devices become more sophisticated and complex, higher reliability is required for electronic devices than before. Therefore, it is required to improve the reliability of electronic devices by improving the cured film and the photosensitive resin composition used to form the cured film. In addition, in recent years, in order to reduce thermal damage to semiconductor chips, it is required to make the heating temperature when forming the cured film relatively low (for example, about 200°C).

[0009] The present invention has been made in view of the above-mentioned technical problems. It has been found that by using a specific phenolic resin, a crosslinking agent and a photosensitizer in combination in a positive photosensitive resin composition, a resin film having low-temperature curing properties and excellent mechanical properties of the cured product can be obtained, resulting in excellent adhesion to the substrate, thereby completing the present invention.

[0010] Means for solving technical problems

[0011] According to the present invention, a positive photosensitive resin composition can be provided, which can be used for a rewiring layer of a semiconductor device, wherein the photosensitive resin composition comprises: (A) a phenolic resin having a biphenol structure; (B) a crosslinking agent; and (C) a photosensitizer, wherein the tensile strength of a cured product obtained by curing the positive photosensitive resin composition at 180° C. is greater than 100 MPa.

[0012] Furthermore, according to the present invention, a cured film obtained by curing the positive photosensitive resin composition can be provided.

[0013] Furthermore, according to the present invention, there can be provided a semiconductor device comprising: a semiconductor element; and a rewiring layer provided on a surface of the semiconductor element, wherein the insulating layer in the rewiring layer is composed of the above-mentioned cured film.

[0014] Effects of the Invention

[0015] According to the present invention, it is possible to provide a positive photosensitive resin composition having low temperature curability and a cured film having excellent mechanical strength obtained by curing the positive photosensitive resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a cross-sectional view showing a structural example of a semiconductor device in an embodiment. DETAILED DESCRIPTION

[0017] The following is a description of the embodiments of the present invention. In addition, in this specification, the numerical range "x to y" means "above x and below y", and both the lower limit x and the upper limit y are included. For example, "1 to 5 mass %" means "above 1 mass % and below 5 mass %". In addition, in the following drawings, the same components are marked with the same reference numerals, and the description is appropriately omitted. In addition, the drawings are schematic diagrams and are inconsistent with the actual dimensional ratios.

[0018] In the description of the group (atomic group) in this specification, the description without description of substitution or unsubstituted includes both the case of having no substituent and the case of having a substituent. For example, "alkyl" includes not only alkyl without substituent (unsubstituted alkyl) but also alkyl with substituent (substituted alkyl).

[0019] [Positive photosensitive resin composition]

[0020] The positive photosensitive resin composition of the present embodiment is a resin material that can be used to form a rewiring layer of a semiconductor device. The positive photosensitive resin composition of the present embodiment comprises (A) a phenolic resin, (B) a crosslinking agent, and (C) a photosensitizer, wherein the phenolic resin (A) is a phenolic resin having a biphenol structure, in other words, a biphenyl type phenolic resin.

[0021] In the positive photosensitive resin composition of the present embodiment, a cured product obtained by curing the positive photosensitive resin composition at 180° C. has a tensile breaking strength of 100 MPa or more.

[0022] The present inventors have conducted research to improve the low-temperature curability of a positive photosensitive resin composition and the mechanical strength of the obtained cured film. As a result, they have found that by adopting a structure in which the positive photosensitive resin composition contains specific components, the tensile strength of a cured product obtained by curing the positive photosensitive resin composition at 180° C. is 100 MPa or more, thereby solving the above-mentioned technical problems.

[0023] Hereinafter, each component used for the positive photosensitive resin composition of this embodiment is demonstrated.

[0024] (Phenolic resin (A))

[0025] The positive photosensitive resin composition of the present embodiment includes a biphenyl phenolic resin (a1) as the phenolic resin. As the biphenyl phenolic resin (a1), from the viewpoint of improving the curability at low temperatures and the reliability of the cured film, a biphenyl phenolic resin having a structural unit having a biphenol skeleton represented by the following formula (2) is preferred.

[0026]

[0027] In the above formula (2), R 41 and R 42 Each is independently a monovalent substituent selected from a hydroxyl group, a halogen atom, a carboxyl group, a saturated or unsaturated alkyl group having 1 to 20 carbon atoms, an alkyl ether group having 1 to 20 carbon atoms, a saturated or unsaturated alicyclic group having 3 to 20 carbon atoms, or an organic group having an aromatic structure having 6 to 20 carbon atoms, which may be bonded via an ester bond, an ether bond, an amide bond, or a carbonyl bond, r and s are each independently an integer of 0 to 3, Y4 and Z4 are each independently selected from a single bond, an aliphatic group having 1 to 10 carbon atoms which may have an unsaturated bond, an aliphatic group having 3 to 20 carbon atoms, and an organic group having an aromatic structure having 6 to 20 carbon atoms, and Z4 is bonded to any one of the two benzene rings.

[0028] In the present embodiment, from the viewpoint of improving curability at low temperatures of 200° C. or lower (e.g., 180° C.), the weight average molecular weight of the biphenyl phenolic resin (a1) is 12,000 or higher, preferably 15,000 or higher, more preferably 18,000 or higher, and further preferably 20,000 or higher. Furthermore, from the viewpoint of maintaining appropriate solvent solubility, the weight average molecular weight of the biphenyl phenolic resin (a1) is 500,000 or lower, preferably 400,000 or lower, more preferably 300,000 or lower, and further preferably 200,000 or lower.

[0029] Specifically, the biphenyl-type phenol resin (a1) having a structural unit represented by formula (2) can be obtained using the method described in JP-A-2018-155938.

[0030] From the viewpoint of improving curability during low-temperature curing, the content of the biphenyl phenolic resin (a1) in the positive photosensitive resin composition of the present embodiment is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more, relative to the total solid content of the positive photosensitive resin composition. Furthermore, from the viewpoint of deterioration of toughness, the content of the biphenyl phenolic resin (a1) in the positive photosensitive resin composition is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less, relative to the total solid content of the positive photosensitive resin composition.

[0031] From the viewpoint of improving the curability at low temperatures and the reliability of the cured film, the positive photosensitive resin composition of the present embodiment may further contain a phenol resin (a2) other than the biphenyl-type phenol resin (a1).

[0032] Specific examples of the phenolic resin (a2) include phenol novolac type phenolic resins such as phenol novolac resins, cresol novolac resins, bisphenol novolac resins, phenol-biphenyl novolac resins, allylated novolac type phenolic resins, and xylene novolac type phenolic resins; reaction products of phenol compounds such as novolac type phenolic resins, resol type phenolic resins, and cresol novolac resins with aldehyde compounds; and reaction products of phenol compounds such as phenol aralkyl resins with dimethylol compounds.

[0033] Among them, the phenol resin (a2) is preferably a resin having a structure represented by the following formula (1) from the viewpoint of obtaining a resin composition having low-temperature curability.

[0034]

[0035] In the above formula (1), from the viewpoint of improving curability at low temperatures, n is preferably 6 or more, more preferably 10 or more, and even more preferably 14 or more.

[0036] Furthermore, from the viewpoint of solvent solubility, n is preferably 72 or less, more preferably 54 or less, and even more preferably 36 or less.

[0037] From the viewpoint of improving curability at low temperatures, the weight average molecular weight of the biphenyl phenolic resin (a2) is, for example, 500 or more, preferably 2000 or more, more preferably 3000 or more, and further preferably 4000 or more. From the viewpoint of solvent solubility, the weight average molecular weight of the biphenyl phenolic resin (a2) is, for example, 50,000 or less, preferably 20,000 or less, more preferably 15,000 or less, and further preferably 10,000 or less.

[0038] When the positive photosensitive resin composition contains a biphenyl phenolic resin (a2), from the viewpoint of improving toughness during low-temperature curing, the content of the biphenyl phenolic resin (a2) is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15 parts by mass or more relative to the total solid content of the positive photosensitive resin composition. Furthermore, from the viewpoint of mechanical properties of the obtained cured film, the content of the biphenyl phenolic resin (a2) in the positive photosensitive resin composition is preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and further preferably 50 parts by mass or less relative to the total solid content of the positive photosensitive resin composition.

[0039] The positive photosensitive resin composition of this embodiment may contain a thermosetting resin other than the phenolic resins (a1) and (a2). Specific examples of such resins include phenolic resins other than the biphenyl-type phenolic resins, hydroxystyrene resins, polyamide resins, polybenzoxazole resins, polyimide resins, and cyclic olefin resins.

[0040] Furthermore, from the viewpoint of improving the curability at low temperatures and the reliability of the cured film, the content of the phenolic resin (A) in the positive photosensitive resin composition is preferably 30% by mass or more, more preferably 45% by mass or more, further preferably 50% by mass or more, and further preferably 55% by mass or more, relative to the total solid content of the photosensitive resin composition. Furthermore, from the viewpoint of improving chemical resistance and photosensitivity, the content of the component (A) in the photosensitive resin composition is preferably 95% by mass or less, more preferably 90% by mass or less, and further preferably 85% by mass or less, relative to the total solid content of the photosensitive resin composition. Among them, the phenolic resin (A) is the total amount of the phenolic resins used in the positive photosensitive resin composition of the present embodiment, and the phenolic resin (A) is composed of the above-mentioned biphenyl type phenolic resin (a1) and the phenolic resin (a2) used as needed.

[0041] (Crosslinking agent (B))

[0042] The positive photosensitive resin composition of the present embodiment contains a crosslinking agent (B) having a reactive group capable of crosslinking with the phenol resin (A). As such a crosslinking agent (B), a bifunctional or higher-functional urea resin-based crosslinking agent (b1) is preferably used.

[0043] Examples of the bifunctional or higher-functional urea resin crosslinking agent (b1) include bifunctional to tetrafunctional alkoxymethylated glycoluril compounds. The alkoxymethylated glycoluril compound refers to a compound in which the hydrogen atom of the amino group of the glycoluril compound is substituted with an alkoxy hydroxymethyl group. Specific examples of the alkoxymethylated glycoluril include 1,3,4,6-tetrakis(methoxymethyl) glycoluril, 1,3,4,6-tetrakis(butoxymethyl) glycoluril, 1,3,4,6-tetrakis(hydroxymethyl) glycoluril, 1,3-bis(hydroxymethyl)urea, 1,1,3,3-tetrakis(butoxymethyl)urea, 1,1,3,3-tetrakis(methoxymethyl)urea, 1,3-bis(hydroxymethyl)-4,5-dihydroxy-2-imidazolidinone, and 1,3-bis(methoxymethyl)-4,5-dimethoxy-2-imidazolidinone.

[0044] The crosslinking agent (B) may contain other crosslinking agents (b2) in addition to the above-mentioned 22- or higher-functional urea resin crosslinking agent (b1) within a range that does not impair the low-temperature curability of the positive photosensitive resin composition. As other crosslinking agents (b2), for example, compounds having hydroxymethyl groups such as 1,2-benzenedimethanol, 1,3-benzenedimethanol, 1,4-benzenedimethanol (p-benzenedimethanol), 1,3,5-benzenetrimethylol, 4,4-biphenyl dimethanol, 2,6-pyridine dimethanol, 2,6-bis(hydroxymethyl)-p-cresol, 4,4′-methylenebis(2,6-dialkoxymethylphenol); phenols such as pentahydroxybiphenyl; compounds having alkoxymethyl groups such as 1,4-bis(methoxymethyl)benzene, 1,3-bis(methoxymethyl)benzene, 4,4′-bis(methoxymethyl)biphenyl, 3,4′-bis(methoxymethyl)biphenyl, 3,3′-bis(methoxymethyl)biphenyl, methyl 2,6-naphthalene dicarboxylate, 4,4′-methylenebis(2,6-dimethoxymethylphenol); hexahydroxymethylmelamine, hexabutanol Methylol melamine compounds represented by melamine, etc.; alkoxy melamine compounds such as hexamethoxy melamine; methylol urea compounds such as methylol benzoguanamine compounds and dimethylol ethylene urea; alkylated urea resins; cyano compounds such as dicyanoaniline, dicyanophenol, and cyanophenylsulfonic acid; isocyanate compounds such as 1,4-phenylene diisocyanate and 3,3′-dimethyldiphenylmethane-4,4′-diisocyanate; compounds containing epoxy groups such as ethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, isocyanuric acid triglycidyl ester, bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene epoxy resin, biphenyl type epoxy resin, phenol novolac resin type epoxy resin; maleimide compounds such as N,N′-1,3-phenylenedimaleimide and N,N′-methylenedimaleimide, etc.

[0045] From the viewpoint of improving the toughness of the positive photosensitive resin composition during low-temperature curing, the content of the difunctional or higher urea resin crosslinking agent (b1) is preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more, relative to the total solid content of the positive photosensitive resin composition. Furthermore, from the viewpoint of maintaining the thermomechanical properties of the positive photosensitive resin composition during low-temperature curing, the content of the difunctional or higher urea resin crosslinking agent (b1) in the positive photosensitive resin composition is preferably 90% by mass or less, more preferably 85% by mass or less, and further preferably 80% by mass or less, relative to the total solid content of the photosensitive resin composition.

[0046] From the viewpoint of improving toughness during low-temperature curing, the content of the crosslinking agent (B) in the positive photosensitive resin composition of the present embodiment is preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more relative to the total solid content of the positive photosensitive resin composition. In addition, from the viewpoint of maintaining thermomechanical properties during low-temperature curing, the content of the crosslinking agent (B) in the positive photosensitive resin composition is preferably 90% by mass or less, more preferably 85% by mass or less, and further preferably 80% by mass or less relative to the total solid content of the positive photosensitive resin composition. Among them, the crosslinking agent (B) is composed of the above-mentioned bifunctional or higher urea resin crosslinking agent (b1) and other crosslinking agents (b2) used as needed.

[0047] (Photosensitive agent (C))

[0048] From the viewpoint of stably forming a cured film, the positive photosensitive resin composition of this embodiment includes a photosensitive agent (C). Specifically, the photosensitive agent (C) is an acid generator that can generate an acid by absorbing heat energy or light energy. From the viewpoint of improving curability and chemical resistance at low temperatures, the photosensitive agent (C) includes either or both of a thermal acid generator (c1) that can generate an acid by heat energy or a photoacid generator (c2) that can generate an acid by light energy.

[0049] As the thermal acid generator (c1), a sulfonium compound or a salt thereof is preferably used.

[0050] Specifically, the sulfonium compound or its salt is a sulfonium salt having a sulfonium ion as a cation portion. In this case, specifically, the anion portion of the sulfonium compound or its salt is a sulfonate ion such as a boride ion, an antimony ion, a phosphorus ion or a trifluoromethanesulfonate ion, and from the viewpoint of increasing the reaction rate at low temperatures, a boride ion or an antimony ion is preferred, and a boride ion is more preferred. These anions may have a substituent.

[0051] The sulfonium compound or its salt preferably contains a sulfonium salt represented by the following formula (4).

[0052]

[0053] In the above general formula (4), R 1 It is a hydrogen atom or a monovalent organic group, and from the viewpoint of improving reactivity at low temperatures, it is preferably a hydrogen atom or an acyl group, more preferably an acyl group, and still more preferably a CH3C(=O) group.

[0054] R 2It is a monovalent organic group, and from the viewpoint of improving reactivity at low temperatures, it is preferably a chain or branched hydrocarbon group or a benzyl group which may have a substituent, more preferably a benzyl group which may be substituted by an alkyl group having 1 to 4 carbon atoms or an alkyl group having 1 to 4 carbon atoms, and still more preferably a methyl group or a benzyl group in which the aromatic ring moiety may be substituted by a methyl group.

[0055] R 3 It is a monovalent organic group, and from the viewpoint of improving reactivity at low temperatures, is preferably a chain or branched hydrocarbon group, more preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group.

[0056] Other preferred examples of the thermal acid generator (c1) include triphenylsulfonium salts such as triphenylsulfonium trifluoromethanesulfonate.

[0057] Examples of the photoacid generator (c2) include naphthoquinonediazide compounds, diarylsulfonium salts, triarylsulfonium salts, dialkylphenacylsulfonium salts, diaryliodonium salts, aryldiazonium salts, aromatic tetracarboxylic acid esters, aromatic sulfonic acid esters, nitrobenzyl esters, aromatic N-oxalimide sulfonates, aromatic sulfonamides, benzoquinonediazoniumsulfonates, etc. Among them, naphthoquinonediazide compounds are preferred.

[0058] Examples of naphthoquinonediazide compounds include naphthoquinonediazide adducts of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene and naphthoquinonediazide adducts of tetrahydroxybenzophenone. The addition of naphthoquinonediazide can be produced by reacting o-quinonediazidesulfonyl chloride with a hydroxy compound or an amino compound.

[0059] From the viewpoint of improving curability at low temperatures, the content of the photosensitive agent (C) in the positive photosensitive resin composition is preferably 3% by mass or more, more preferably 5% by mass or more, and further preferably 8% by mass or more, relative to the total solid content of the positive photosensitive resin composition. In addition, from the viewpoint of suppressing a decrease in reliability, the content of the photosensitive agent (C) in the positive photosensitive resin composition is preferably 20% by mass or less, more preferably 18% by mass or less, and further preferably 16 parts by mass or less, relative to the total solid content of the photosensitive resin composition. The photosensitive agent (C) is composed of a thermal acid generator (c1) and / or a photoacid generator (c2).

[0060] The positive photosensitive resin composition of the present embodiment preferably contains the above-mentioned thermal acid generator (c1) and photoacid generator (c2) in combination as the photosensitive agent (C). As a result, the mechanical strength of the cured product of the obtained positive photosensitive resin composition can be improved. When the photosensitive resin composition contains the thermal acid generator (c1) and the photoacid generator (c2) in combination, the thermal acid generator (c1): photoacid generator (c2) expressed as a mixing ratio converted into their mass ratio is, for example, 2:8 to 8:2, preferably 3:7 to 7:3, and more preferably 4:6 to 6:4.

[0061] (Flexible epoxy resin (D))

[0062] The positive photosensitive resin composition of this embodiment preferably contains a flexible epoxy resin (D). As a result, the cured product of the photosensitive resin composition can have a tensile strength at break within a desired range. As the flexible epoxy resin (D), an epoxy resin (d1) containing an alkylene structure having an ether bond and having 4 or more carbon atoms is preferably used.

[0063] The flexible epoxy resin (d1) is preferably a compound in which a part or all of the epoxy resin has a flexible structure selected from an alkylene structure having 2 to 20 carbon atoms and an alkylene structure having 2 to 20 carbon atoms and an ether bond. Examples of such flexible epoxy resins (d1) include EXA-4850-150, EXA-4816 and EXA-4822 manufactured by DIC Corporation (epoxy resins containing an alkylene structure having an ether bond); EP-4000S, EP-4000SS, EP-4003S, EP-4010S and EP-4011S manufactured by ADEKA CORPORATION (epoxy resins containing an alkylene structure having an ether bond); BEO-60E and BPO-20E manufactured by New Japan Chemical Co., Ltd. (epoxy resins containing an alkylene structure having an ether bond); and Mitsubishi Chemical Corporation. Corporation) YX7105, YX7110 and YX7400 (epoxy resin containing an alkylene structure having an ether bond) and YX7180 (phenoxy resin containing an alkylene structure having an ether bond) etc. The flexible epoxy resin (d1) may be used alone or in combination of two or more.

[0064] When a flexible epoxy resin (d1) is used, the content of the flexible epoxy resin (d1) in the positive photosensitive resin composition is preferably 3% by mass or more, more preferably 5% by mass or more, and further preferably 10% by mass or more, relative to the total solid content of the positive photosensitive resin composition, from the viewpoint of improving toughness during low-temperature curing. Furthermore, from the viewpoint of maintaining thermomechanical properties during low-temperature curing, the content of the flexible epoxy resin (d1) in the positive photosensitive resin composition is preferably 60% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less, relative to the total solid content of the photosensitive resin composition.

[0065] The positive photosensitive resin composition of this embodiment may contain other epoxy resins (d2) other than the above-mentioned epoxy resin (d1). Examples of other epoxy resins (d2) include bisphenol A type phenoxy resins, bisphenol F type phenoxy resins, bisphenol S type phenoxy resins, bisphenol acetophenone type phenoxy resins, novolac type phenoxy resins, biphenyl type phenoxy resins, fluorene type phenoxy resins, dicyclopentadiene type phenoxy resins, norbornene type phenoxy resins, naphthalene type phenoxy resins, anthracene type phenoxy resins, adamantane type phenoxy resins, terpene type phenoxy resins, and trimethylcyclohexane type phenoxy resins.

[0066] (Sealing agent (E))

[0067] The positive photosensitive resin composition of this embodiment preferably contains an adhesion aid (E). Thereby, for example, the adhesion with the substrate can be further improved.

[0068] The adhesion aid (E) is not particularly limited. For example, silane coupling agents such as amino-containing silane coupling agents, epoxy-containing silane coupling agents, (meth)acryloyl-containing silane coupling agents, mercapto-containing silane coupling agents, vinyl-containing silane coupling agents, urea-containing silane coupling agents, and sulfide-containing silane coupling agents can be used.

[0069] When using a silane coupling agent, one type may be used alone, or two or more types may be used simultaneously.

[0070] Examples of the amino group-containing silane coupling agent include bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)γ-aminopropyltrimethoxysilane, N-β (aminoethyl)γ-aminopropyltriethoxysilane, N-β (aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)γ-aminopropylmethyldiethoxysilane, and N-phenyl-γ-amino-propyltrimethoxysilane.

[0071] Examples of the epoxy group-containing silane coupling agent include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane.

[0072] Examples of the (meth)acryloyl group-containing silane coupling agent include γ-((meth)acryloxypropyl)trimethoxysilane, v-((meth)acryloxypropyl)methyldimethoxysilane, and γ-((meth)acryloxypropyl)methyldiethoxysilane.

[0073] Examples of the mercapto group-containing silane coupling agent include 3-mercaptopropyltrimethoxysilane and the like.

[0074] Examples of the vinyl group-containing silane coupling agent include vinyl tris(β-methoxyethoxy)silane, vinyl triethoxysilane, and vinyl trimethoxysilane.

[0075] Examples of the urea group-containing silane coupling agent include 3-ureidopropyltriethoxysilane and the like.

[0076] Examples of the sulfide group-containing silane coupling agent include bis(3-(triethoxysilyl)propyl)disulfide and bis(3-(triethoxysilyl)propyl)tetrasulfide.

[0077] Examples of the acid anhydride-containing silane coupling agent include 3-trimethoxysilylpropylsuccinic anhydride, 3-triethoxysilylpropylsuccinic anhydride, and 3-dimethylmethoxysilylpropylsuccinic anhydride.

[0078] Examples of the adhesion aid include not only silane coupling agents but also titanium coupling agents, zirconium coupling agents, and the like.

[0079] When using an adhesion aid, one type of adhesion aid may be used alone, or two or more types of adhesion aids may be used simultaneously.

[0080] When using an adhesion aid, the content of the adhesion aid is preferably 0.3 to 15 parts by mass, more preferably 0.4 to 12 parts by mass, and even more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the phenolic resin (A).

[0081] (Surfactant)

[0082] The positive photosensitive resin composition of this embodiment may contain a surfactant. By containing a surfactant, wettability during coating can be improved, and a uniform resin film and cured film can be obtained. Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, alkyl-based surfactants, and acrylic-based surfactants.

[0083] The surfactant preferably includes a surfactant containing at least one of a fluorine atom and a silicon atom. Thus, in addition to being able to obtain a uniform resin film (improving coating properties), being able to improve developability, it is also possible to contribute to improving bonding strength. As such a surfactant, for example, it is preferably a nonionic surfactant containing at least one of a fluorine atom and a silicon atom. Examples of commercially available surfactants include "MEGAFACE" series manufactured by DIC Corporation, F-251, F-253, F-281, F-430, F-477, F-551, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-562, F-563, F-565, F-568, F-569, F-570, F-572, F-574, F-575, F-576, R-40, R-40-LM, R-41, R-94 and other fluorine-containing oligomeric surfactants, and Ftergent manufactured by NEOS COMPANY LIMITED. Fluorinated nonionic surfactants such as SULFATE 250 and FTERGENT 251, and silicone surfactants such as the SILFOAM (registered trademark) series manufactured by Wacker Chemie AG (for example, SD 100TS, SD 670, SD 850, SD 860, and SD 882).

[0084] When the positive photosensitive resin composition contains a surfactant, the photosensitive resin composition may contain one or more surfactants.

[0085] When the photosensitive resin composition contains a surfactant, the amount of the surfactant is, for example, 0.001 to 1 part by mass, or preferably 0.005 to 0.5 parts by mass, relative to 100 parts by mass of the phenol resin (A).

[0086] (Solvent)

[0087] The positive photosensitive resin composition of this embodiment preferably contains a solvent. Thus, a photosensitive resin film can be easily formed on the step substrate by a coating method. When the positive photosensitive resin composition of this embodiment contains a solvent, the positive photosensitive resin composition of this embodiment is, for example, in the form of a varnish.

[0088] The solvent generally includes an organic solvent. The organic solvent is not particularly limited as long as it can dissolve or disperse the above-mentioned components and does not substantially chemically react with the constituent components.

[0089] Examples of the organic solvent include acetone, methyl ethyl ketone, toluene, propylene glycol methyl ethyl ether, propylene glycol dimethyl ether, propylene glycol 1-monomethyl ether 2-acetate, diethylene glycol ethyl methyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol dimethyl ether, n-butyl ether acetate, benzyl alcohol, propylene carbonate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, butyl acetate, and γ-butyrolactone. These may be used alone or in combination of a plurality of them.

[0090] When a solvent is used, the non-volatile component concentration in the positive photosensitive resin composition is preferably 30 to 75% by mass, more preferably 35 to 70% by mass. Within this range, each component can be fully dissolved or dispersed. In addition, good coating properties can be ensured, and the flatness during spin coating can be optimized. In addition, by adjusting the content of the non-volatile component, the viscosity of the positive photosensitive resin composition can be appropriately controlled.

[0091] (Other ingredients)

[0092] The positive photosensitive resin composition of the present embodiment may contain components other than the above components as necessary, in addition to the above components. Examples of such components include antioxidants, fillers such as silica, sensitizers, and film-forming agents.

[0093] (Characteristics of positive photosensitive resin composition)

[0094] The positive photosensitive resin composition of the present embodiment includes the above-mentioned components, and thus the tensile breaking strength of a cured product obtained by curing the positive photosensitive resin composition at 180° C. can be 100 MPa or more.

[0095] From the viewpoint of suppressing brittle fracture, the lower limit of the tensile strength at break of the cured film of the positive photosensitive resin composition of the present embodiment is 100 MPa or more, preferably 105 MPa or more, and more preferably 110 MPa or more. From the viewpoint of obtaining a cured film more stably, the upper limit of the tensile strength at break of the cured film is, for example, 200 MPa or less, preferably 180 MPa or less, and more preferably 150 MPa or less.

[0096] The positive photosensitive resin composition of the present embodiment can contain the above-mentioned components, so that the tensile elongation of a cured film of the positive photosensitive resin composition measured under the following condition 1 is 20% or more.

[0097] (Condition 1)

[0098] (i) The positive photosensitive resin composition was cured at 200° C. for 180 minutes to form the cured film, and a sample having a size of 6.5 mm×20 mm×10 μm was prepared from the cured film.

[0099] (ii) According to JIS K7161, a tensile test of the sample was carried out at 23° C. and a test speed of 5 mm / min to determine the tensile elongation.

[0100] From the viewpoint of suppressing brittle fracture, the lower limit of the tensile elongation of the cured film of the positive photosensitive resin composition of the present embodiment is 20% or more, preferably 25% or more, more preferably 30% or more, and further preferably 40% or more. Furthermore, from the viewpoint of obtaining a cured film more stably, the upper limit of the tensile elongation of the cured film is 100% or less, preferably 190% or less, more preferably 80% or less, and further preferably 70% or less.

[0101] In this embodiment, from the viewpoint of improving heat resistance, the glass transition temperature (Tg) of the cured product of the positive photosensitive resin composition is preferably 200° C. or higher, and more preferably 220° C. or higher. Furthermore, from the viewpoint of suppressing deterioration of brittleness, the glass transition temperature of the cured product of the positive photosensitive resin composition is preferably 300° C. or lower, more preferably 280° C. or lower, and further preferably 260° C. or lower.

[0102] The Tg of the cured product of the positive photosensitive resin composition is calculated based on the results of measuring a specified test piece (width 3 mm × length 10 mm × thickness 0.005 to 0.015 mm) using a thermomechanical analyzer (TMA) under the conditions of a starting temperature of 30°C, a measuring temperature range of 30 to 440°C, and a heating rate of 10°C / min.

[0103] [Curing resin film]

[0104] The resin film is obtained by curing the photosensitive resin composition in this embodiment. In addition, the resin film in this embodiment is a dried film or a cured film of the photosensitive resin composition. That is, the resin film is formed by drying or curing the photosensitive resin composition, preferably by curing the photosensitive resin composition.

[0105] The resin film can be used to form a permanent film, a resin film for electronic devices such as a resist, etc. Among them, the use of forming a permanent film is preferred from the viewpoint of being able to obtain a resin film at a low temperature, having excellent processability, and being able to obtain a resin film with excellent reliability.

[0106] According to the present embodiment, for example, a resin film obtained using the photosensitive resin composition can also be obtained, which has excellent processability and reliability required as a resin film useful for producing electronic devices or the like.

[0107] The permanent film is composed of a resin film obtained by pre-baking, exposing and developing a photosensitive resin composition, patterning it into a desired shape, and then post-baking it to cure it. The permanent film can be used as a protective film for electronic devices such as a buffer coating film, an interlayer film such as a rewiring insulating film, a dam material, etc.

[0108] The resist is composed of a resin film obtained by applying a negative photosensitive resin composition to an object to be shielded by the resist by a method such as spin coating, roll coating, flow coating, dip coating, spray coating, or doctor blade coating, and removing a solvent from the negative photosensitive resin composition.

[0109] Figure 1 It is a cross-sectional view showing a structural example of an electronic device including the resin film in this embodiment.

[0110] Figure 1 The electronic device 100 shown may be an electronic device including the above-mentioned resin film. Specifically, at least one of the passivation film 32, the insulating layer 42 and the insulating layer 44 in the electronic device 100 may be a resin film. The resin film is preferably the above-mentioned permanent film.

[0111] The electronic device 100 is, for example, a semiconductor chip. In this case, for example, a semiconductor package can be obtained by mounting the electronic device 100 on a wiring substrate via the bumps 52. The electronic device 100 includes: a semiconductor substrate provided with semiconductor elements such as transistors; and a multilayer wiring layer (not shown) provided on the semiconductor substrate. In the uppermost layer of the multilayer wiring layer, an interlayer insulating film 30 and an uppermost wiring 34 provided on the interlayer insulating film 30 are provided. The uppermost wiring 34 is made of, for example, aluminum Al. In addition, a passivation film 32 is provided on the interlayer insulating film 30 and on the uppermost wiring 34. In a portion of the passivation film 32, an opening is provided to expose the uppermost wiring 34.

[0112] A rewiring layer 40 is provided on the passivation film 32. The rewiring layer 40 includes: an insulating layer 42 provided on the passivation film 32; a rewiring 46 provided on the insulating layer 42; and an insulating layer 44 provided on the insulating layer 42 and on the rewiring 46. An opening connected to the uppermost wiring 34 is formed in the insulating layer 42. The rewiring 46 is formed on the insulating layer 42 and in the opening provided in the insulating layer 42, and is connected to the uppermost wiring 34. An opening connected to the rewiring 46 is provided in the insulating layer 44.

[0113] Bumps 52 are formed in the openings provided in the insulating layer 44 via, for example, an Under Bump Metallurgy (UBM) layer 50. The electronic device 100 is connected to a wiring board or the like via the bumps 52, for example.

[0114] As mentioned above, although embodiment of this invention was demonstrated, these are illustrations of this invention, and various structures other than the above-mentioned can also be adopted.

[0115] Example

[0116] Hereinafter, the present invention will be described with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0117] (Examples 1 to 7, Comparative Example 1)

[0118] A photosensitive resin composition was prepared according to the formulation described in Table 1. Specifically, first, the components formulated according to Table 1 were stirred and mixed under a nitrogen atmosphere, and then filtered through a polyethylene filter with a pore size of 0.2 μm to obtain a varnish-like photosensitive resin composition. The details of the components described in Table 1 are shown below.

[0119] (Phenolic resin (A))

[0120] (Biphenyl type phenolic resin (a1))

[0121] Phenolic resin a1-1: a biphenyl-type phenolic resin having the formula (a1-1) produced by the following method, manufactured by Sumitomo Bakelite Co., Ltd., PR-X21024, Mw=45000

[0122] (Manufacture of phenolic resin a1-1)

[0123] After adding 4,4'-biphenol 186.2g (1.00mol), p-cresol 86.5g (0.8mol), formaldehyde 28.5g (0.94mol), p-toluenesulfonic acid 15.5g (0.09mol) and 308g of γ-butyrolactone into a glass round-bottom flask having four ports including a thermometer, a stirrer, a raw material inlet and a dry nitrogen inlet tube, the reaction solution was refluxed in the round-bottom flask in an oil bath while nitrogen was flowing, and a polycondensation reaction was performed at 100°C for 5.5 hours. Then, after the obtained reaction solution was cooled to room temperature, 411g of acetone was added and stirred and mixed until uniform. After that, the reaction solution in the round-bottom flask was dripped and mixed into 10L of water to precipitate the resin component. Then, after filtering and recovering the precipitated resin component, it was vacuum dried at 60°C to obtain a phenolic resin represented by the following formula (a1-1). The weight average molecular weight of the obtained phenol resin (a1-1) was 45,000.

[0124]

[0125] Phenolic resin a1-2: Biphenyl phenolic resin having the formula (a1-2) produced by the following method, manufactured by Sumitomo Bakelite Co., Ltd., Mw=45000

[0126] (Manufacture of phenolic resin a1-1)

[0127] After adding 4,4'-biphenol 186.2g (1.00mol), p-cresol 86.5g (0.8mol), formaldehyde 24.0g (0.8mol), oxalic acid dihydrate 11.3g (0.09mol) and 308g of γ-butyrolactone into a glass round-bottom flask having four ports including a thermometer, a stirrer, a raw material inlet and a dry nitrogen inlet tube, the reaction solution was refluxed in the round-bottom flask in an oil bath while nitrogen was flowing, and a polycondensation reaction was performed at 100°C for 6 hours. Then, after the obtained reaction solution was cooled to room temperature, 411g of acetone was added and stirred and mixed until uniform. After that, the resin component was precipitated by adding the reaction solution in the round-bottom flask dropwise to 10L of water. Then, the precipitated resin component was filtered and recovered, and then vacuum dried at 60°C to obtain a phenolic resin represented by the following formula (a1-2). The weight average molecular weight of the obtained phenol resin (a1-2) was 11,000.

[0128]

[0129] (Crosslinking agent (B))

[0130] (Urea resin crosslinking agent (b1))

[0131] Crosslinking agent b1-1: 1,3,4,6-tetrakis(methoxymethyl)glycoluril, manufactured by DAITO CHEMIX Co., Ltd., CROLIN-318

[0132] Crosslinking agent b1-2: 1,3,4,6-tetrakis(butoxymethyl)glycoluril, manufactured by Sanwa Chemical Co., Ltd., NIKALAC MX-279

[0133] Crosslinking agent b1-3: 1,3-bis(methoxymethyl)-4,5-dimethoxy-2-imidazolidinone, manufactured by Sanwa Chemical Co., Ltd., NIKALAC MX-280

[0134] (Epoxy resin crosslinking agent (b2))

[0135] Crosslinking agent b2-1: phenoxy epoxy resin, manufactured by Mitsubishi Chemical Corporation, YX-7105

[0136] Crosslinking agent b2-2: Epoxy resin (bisphenol A type phenoxy), manufactured by Mitsubishi Chemical Corporation, JER-1256

[0137] Crosslinking agent b2-3: Bisphenol A type epoxy resin, manufactured by OSAKASODA CO., LTD., LX-01

[0138] (Photosensitive agent (C))

[0139] (Thermal acid generator (c1))

[0140] Thermal acid generator c1-1: a compound represented by the formula (c1-1) (manufactured by Sanshin Chemical Industry Co., Ltd., SAN-AID SI-150)

[0141]

[0142] (Photoacid generator (c2))

[0143] Photoacid generator c2-1: 3-diazo-3,4-dihydro-4-oxo-1-naphthalenesulfonate of 4,4′-(1-{4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl}ethylidene)diphenol, manufactured by DAITO CHEMIX Co., Ltd., DS-427

[0144] (Sealing aid)

[0145] Adhesion aid 1: 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., KBM-403E

[0146] (Surfactant)

[0147] Surfactant 1: Fluorine-based surfactant, manufactured by 3M Japan Limited, FC4432 (10% GBL)

[0148] (Solvent)

[0149] Solvent 1: γ-butyrolactone, manufactured by SANWAYUKA INDUSTRYCORPORATION

[0150] The following physical properties of the obtained resin composition were measured.

[0151] (Low temperature curing property (curing temperature))

[0152] The photosensitive resin composition obtained above was spin-coated on an 8-inch silicon wafer in such a manner that the film thickness after drying was 10 μm, and was cured by heat treatment in an inert oven (manufactured by Koyo Thermo Systems Co., Ltd., product model CLH-21CD-(V)-S) under a nitrogen atmosphere according to the following temperature setting and internal temperature measurement. The curing temperature is shown in Table 1.

[0153] 180℃ curing: room temperature (30℃) → 30 minutes to raise the temperature to 180℃ → maintain at 180℃ for 2 hours → 30 minutes to cool down to room temperature

[0154] (Tensile elongation at break)

[0155] The photosensitive resin composition obtained in each example was cured at 180° C. for 120 minutes to form a cured film. A test piece having a size of 6.5 mm×20 mm×10 μm in thickness was prepared from the obtained cured film.

[0156] According to JIS K7161, the tensile test of the sample was carried out under the conditions of 23°C and a test speed of 5 mm / min using a tensile tester (Tensilon RTA-100) manufactured by ORIENTEC CO., LTD. The measurement was performed 8 times for one sample, and the average value ("ave." in Table 1) was taken as the tensile elongation (%). The results are shown in Table 1.

[0157] (Fracturing stress)

[0158] The test piece was subjected to a tensile test (tensile speed: 5 mm / min) in an atmosphere at 23° C. using a tensile tester (Tensilon RTC-1210A) manufactured by ORIENTEC Co., Ltd. The film strength (MPa) was calculated from the strength at film breakage. The results are shown in Table 1.

[0159] (Glass transition temperature (Tg), coefficient of linear expansion (CTE))

[0160] A cured film of the photosensitive resin composition obtained in each example was produced under the conditions of 180° C. for 120 minutes, and a test piece of 3 mm in width×10 mm in length×10 mm in thickness was obtained from the obtained cured film.

[0161] The test piece of each example was measured using a thermomechanical analyzer (TMA, manufactured by Seiko Instruments Inc., SS6000) under the conditions of a starting temperature of 30°C, a measurement temperature range of 30 to 440°C, and a heating rate of 10°C / min, and Tg (°C) and a linear expansion coefficient (ppm / °C) in a temperature range of 50 to 100°C were obtained from the measurement results. The results are shown in Table 1.

[0162] (Developability)

[0163] The photosensitive resin composition obtained above was applied to an 8-inch silicon wafer using a spin coater, and then pre-baked at 100° C. for 4 minutes using a hot plate to obtain a coating film with a thickness of about 6.0 μm. The coating film was irradiated with varying exposure amounts using an i-line stepper (Nikon Corporation, NSR-4425i) through a mask manufactured by TOPPAN INC. (Test pattern No. 1: a residual pattern and a removal pattern with a width of 0.88 to 50 μm were drawn).

[0164] Next, a 2.38% tetramethylammonium hydroxide aqueous solution was used as a developer, and the development time was adjusted so that the difference between the film thickness after pre-baking and the film thickness after development was 1.0 μm. After performing two spin-over immersion developments to dissolve and remove the exposed part, the film was rinsed with pure water for 10 seconds. The minimum exposure dose of +100 mJ / cm2 was used to form a 100 μm square via hole pattern. 2 The resolution of the line pattern was evaluated by exposing the pattern with an energy of . Regarding the resolution, it was confirmed whether there was an opening in the line pattern with a spacing of 10 μm. The evaluation was "A" in the case of an opening, and "B" in the case of no opening, and the results are shown in Table 1.

[0165]

[0166] This application claims priority based on Japanese patent application No. 2022-048073, filed on March 24, 2022, the disclosure of which is incorporated herein in its entirety.

[0167] Description of Reference Numerals

[0168] 30 interlayer insulating film, 32 passivation film, 34 uppermost wiring layer, 40 redistribution wiring layer, 42, 44 insulating layers, 46 redistribution wiring, 50 UBM layer, 52 bump, 100 electronic device.

Claims

1. A positive photosensitive resin composition, which can be used for a rewiring layer of a semiconductor device, wherein the positive photosensitive resin composition is characterized in that: The photosensitive resin composition comprises: (A) a phenolic resin having a biphenol structure; (B) a cross-linking agent; and (C) photosensitizer, The tensile breaking strength of a cured product obtained by curing the positive photosensitive resin composition at 180° C. is 100 MPa or more.

2. The positive photosensitive resin composition according to claim 1, Features: The tensile elongation of a cured product obtained by curing the positive photosensitive resin composition at 180° C. is 20% or more.

3. The positive photosensitive resin composition according to claim 1 or 2, Features: The glass transition temperature of a cured product obtained by curing the positive photosensitive resin composition at 180° C. is 200° C. to 300° C. inclusive.

4. The positive photosensitive resin composition according to any one of claims 1 to 3, Features: The weight average molecular weight of the phenolic resin (A) having a biphenol structure is 12,000 to 500,000.

5. The positive photosensitive resin composition according to any one of claims 1 to 4, Features: The (B) cross-linking agent comprises 1,3,4,6-tetrakis(methoxymethyl)glycoluril.

6. The positive photosensitive resin composition according to any one of claims 1 to 5, Features: The invention further comprises (D) a flexible epoxy resin.

7. The positive photosensitive resin composition according to claim 6, Features: The (D) flexible epoxy resin is an epoxy resin containing an alkylene structure having an ether bond and having 4 or more carbon atoms.

8. The positive photosensitive resin composition according to any one of claims 1 to 7, Features: The invention further comprises (E) a close-fitting auxiliary agent.

9. The positive photosensitive resin composition according to any one of claims 1 to 8, Features: The (C) photosensitizer comprises a thermal acid generator, a photoacid generator or a combination thereof.

10. A cured film, Features: The method is obtained by curing the positive photosensitive resin composition according to any one of claims 1 to 9.

11. A semiconductor device, It is characterized in that include: Semiconductor components; and A rewiring layer is provided on the surface of the semiconductor element, The insulating layer in the rewiring layer is composed of the cured film according to claim 10 .