Method and device for concentrating and crystallizing salt solution

By using dispersants and homoionic acids in the treatment of high-salt wastewater, the problem that moisture and particle size indexes cannot meet expectations during crystallization are solved, efficient separation and simplification of the process, and the particle size of the salt is improved and Purity reduces energy consumption.

CN118925268APending Publication Date: 2024-11-12GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410980944.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing high-salt wastewater treatment technology, the crystallization process lacks effective control, resulting in the moisture and particle size index of the crystallized salt not meeting expectations, increasing the process and energy consumption, and reducing the utilization efficiency of production costs.

Method used

By mixing the salt solution with a dispersant and homoionic acid, aging and solid-liquid separation are performed to control the growth of crystals and solid moisture content, reducing impurity inclusions, and improving particle size and purity.

Benefits of technology

It realizes efficient separation of solids, controls the solid moisture content and particle size, reduces impurity inclusions, simplifies the process, improves the advantages and rationality of the overall process, and reduces subsequent drying needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925268A_ABST
    Figure CN118925268A_ABST
Patent Text Reader

Abstract

The invention discloses a method and a device for concentrating and crystallizing a salt solution, and the method for concentrating and crystallizing the salt solution comprises the following steps: concentrating the salt solution to obtain a concentrated salt solution, and mixing the concentrated salt solution with a dispersing agent and ionic acid to obtain a mixed solution; carrying out aging and solid-liquid separation on the mixed solution to obtain industrial salt; wherein the same ion acid is an acid which is the same as anions of the industrial salt. According to the method, the dispersing agent and the ionic acid are added into the mixed solution, so that normal growth of the crystals is promoted, the solids are efficiently separated, the water content and the particle size of the solids are controlled, and the qualified industrial salt is obtained, and the crystals are large in grain, high in growth speed, low in water content of the solids and low in impurity inclusion; and the overall process advantages and rationality are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-salt wastewater treatment, and in particular to a method and device for concentrating and crystallizing a salt solution. Background Art

[0002] In the chemical production process, saline wastewater is often generated. The treatment of saline wastewater is mainly through concentration (thermal or membrane method) to reduce the amount, and then through thermal evaporation, salt separation and crystallization to utilize the wastewater as a resource.

[0003] At present, mechanical vapor recompression (MVR) technology is the most advanced and energy-saving technology. There are many MVR cases in public use, but often no effective control measures are taken during the crystallization process, so that the quality indicators of the obtained crystallized salt, moisture content and particle size cannot meet expectations. At present, there are technologies that use heat exchangers, evaporation tanks, insulation tanks, crystallization tanks and centrifugal separation equipment to treat high-salt wastewater, which can achieve 30-60 times concentration and derive composite salts. However, the composite salts need to be separated and dried before they can be obtained as industrial finished salts. Drying increases the process and energy consumption, which is not conducive to reducing production costs.

[0004] In summary, how to simplify the process and improve the quality of crystalline salt is very important for the resource utilization of high-salt wastewater. Summary of the invention

[0005] The object of the present invention is to provide a method and device for concentrating and crystallizing a salt solution, thereby increasing the particle size of crystal particles and reducing the water and impurities contained in the product.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for concentrating and crystallizing a salt solution.

[0008] The method comprises: concentrating a salt solution to obtain a concentrated salt solution, mixing the concentrated salt solution with a dispersant and a common ion acid to obtain a mixed solution; aging and solid-liquid separation of the mixed solution to obtain industrial salt;

[0009] Wherein, the common ion acid is an acid having the same anion as the industrial salt.

[0010] In an optional embodiment, the mass fraction of the dispersant in the mixed solution is 5wt%-20wt%;

[0011] and / or, the dispersant is an alcohol or a ketone;

[0012] In an optional embodiment, the mass fraction of the common ion acid in the mixed solution is 5wt%-20wt%;

[0013] And / or, 20% to 60% of the volume of the concentrated salt solution is mixed with a dispersant and a common ion acid to obtain a mixed solution, and the remaining concentrated salt solution is mixed with the salt solution and then concentrated again.

[0014] In an optional embodiment, the aging is carried out in a thickener, the aging time is 0.5h-2h, and the aging temperature is 50°C-80°C;

[0015] And / or, the concentration temperature is 80°C-90°C.

[0016] In an optional embodiment, the salt solution is at least one of a lithium precipitation mother liquor, a raffinate produced in a lithium extraction process, and a high-boron solution produced in a lithium extraction process from a salt lake;

[0017] And / or, the concentrated salt solution is a saturated solution of industrial salt.

[0018] In a second aspect, the present invention provides a device for use in the method for concentrating and crystallizing a salt solution as described in the aforementioned embodiment, comprising an evaporator, the evaporator being provided with a salt solution inlet and a concentrated salt solution outlet, the concentrated salt solution outlet being sequentially connected to a disperser, a thickener and a solid-liquid separation device, the disperser being provided with a feeding device for adding a dispersant and a common ion acid.

[0019] In an optional embodiment, the evaporator includes a heat exchanger and a separator, the salt solution inlet is arranged on the heat exchanger, a heat exchange solution outlet is arranged on the top of the heat exchanger, the heat exchange solution outlet is connected to the heat exchange solution inlet of the separator, the concentrated salt solution outlet is arranged at the bottom of the separator, and the concentrated salt solution outlet is respectively connected to the heat supplement inlet located at the bottom of the heat exchanger and the liquid inlet of the disperser.

[0020] In an optional embodiment, a liquid return inlet is provided on the salt leg of the separator, the supernatant outlet of the thickener is connected to the liquid return inlet, and the solid phase outlet of the thickener is connected to the solid-liquid separation device.

[0021] In an optional embodiment, a low-pressure steam outlet is provided at the top of the separator, a secondary steam inlet is provided on the heat exchanger, the low-pressure steam outlet is connected to the secondary steam inlet through a steam pipe, and a spray tower and a compressor are also connected in series to the steam pipe.

[0022] In an optional embodiment, a preheater for preheating the salt solution is connected in front of the heat exchanger.

[0023] The present invention has the following beneficial effects:

[0024] In the embodiment of the present invention, adding a dispersant and a common ion acid to the mixed liquid is beneficial to promoting the normal growth of crystals, so as to efficiently separate solids, and control the water content and particle size of the solids to obtain qualified industrial salt. In the method of the present invention, the crystal grains are large, the growth rate is fast, the water content of the solids is low, and the impurity inclusions are reduced, thereby improving the overall process advantages and rationality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 It is a schematic diagram of the structure of the salt solution concentration and crystallization device in the present invention.

[0027] Diagram: 1-raw liquid storage tank; 2-preheater; 3-heat exchanger; 4-separator; 5-spray tower; 6-compressor; 7-disperser; 8-thickener; 9-centrifuge; 10-mother liquid storage tank; 11-evaporator. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0029] The embodiment of the present invention provides a method for concentrating and crystallizing a salt solution.

[0030] The method comprises: concentrating a salt solution to obtain a concentrated salt solution, mixing the concentrated salt solution with a dispersant and a common ion acid to obtain a mixed solution; aging and solid-liquid separation of the mixed solution to obtain industrial salt;

[0031] Wherein, the common ion acid is an acid having the same anion as the industrial salt.

[0032] In the embodiment of the present invention, adding a dispersant and a common ion acid to the mixed solution is beneficial to promoting normal growth of crystals.

[0033] (1) Adding a dispersant to the mixed solution helps to reduce the interfacial surface tension, prevent particle agglomeration during the subsequent aging process, and reduce the inclusion of impurity ions in industrial salt.

[0034] (2) Adding common ion acid to the mixed solution is beneficial to reducing the solubility of industrial salt, causing the crystals to grow continuously during the aging process, which is beneficial to increasing the particle size of industrial salt.

[0035] The present invention can efficiently separate solids and control the moisture content and particle size of the solids to obtain qualified industrial salt. In the method of the present invention, the crystal grains are large, the growth rate is fast, the moisture content of the solids is low, and the impurity inclusions are reduced, thereby improving the overall process advantages and rationality.

[0036] In the embodiment of the present invention, only solid-liquid separation such as centrifugation is required to obtain industrial salt with a low water content, and the industrial salt can be discharged without the need for additional drying.

[0037] In some embodiments, the mass fraction of the dispersant in the mixed solution is 5wt%-20wt%, specifically 5wt%, 10wt%, 15wt%, 20wt% or any value between 5wt% and 20wt%. Adding too much dispersant will result in an excessively high content of dispersant in the industrial salt, which will in turn reduce the purity of the industrial salt.

[0038] In some embodiments, the dispersant is an alcohol or a ketone, specifically polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, etc. The raw materials are easily available and the cost is low.

[0039] In some embodiments, the mass fraction of the common ion acid in the mixed solution is 5wt%-20wt%, specifically 5wt%, 10wt%, 15wt%, 20wt% or any value between 5wt% and 20wt%.

[0040] Specifically, when the industrial salt is a chloride salt, the common ion acid can be hydrochloric acid; when the industrial salt is a sulfate salt, the common ion acid can be sulfuric acid; when the industrial salt is a phosphate salt, the common ion acid can be phosphoric acid. The addition of common ion acid is conducive to the forward movement of the precipitation reaction, but too much common ion acid will also lead to a too fast precipitation rate, thereby increasing the amount of impurities and reducing the purity of the industrial salt.

[0041] In some embodiments, 20%-60% of the volume of the concentrated salt solution is mixed with a dispersant and a common ion acid to obtain a mixed solution, and the remaining concentrated salt solution is mixed with the salt solution and then concentrated again. The partial return of the concentrated salt solution can increase the solute content of the solution to be concentrated to increase the crystallization rate, and on the other hand, it can provide crystal seeds for the solution to be concentrated.

[0042] In some embodiments, the aging is carried out in the thickener 8, the aging time is 0.5h-2h, specifically 0.5h, 1h, 1.5h, 2h or any value between 0.5h-2h, and the aging temperature is 50°C-80°C, specifically 50°C, 60°C, 70°C, 80°C or any value between 50°C-80°C. Ensuring a certain time is conducive to ensuring the output of industrial salt, and aging in the thickener 8 is conducive to improving the aging efficiency.

[0043] In some embodiments, the concentration temperature is 80°C-90°C.

[0044] In some embodiments, the salt solution is at least one of a lithium precipitation mother liquor, a raffinate produced in a lithium extraction process, and a high-boron solution produced in a lithium extraction process from a salt lake. When treating high-salt wastewater commonly discharged from industry, the main purpose is to reduce the content of impurities in the treated wastewater. After the lithium precipitation mother liquor is crystallized to obtain industrial salt, the liquid phase will be returned to the system to recover the lithium element therein. Therefore, it is necessary to reduce the impurities in the industrial salt, especially the inclusion of lithium ions.

[0045] In some embodiments, the concentrated salt solution is a saturated solution of industrial salt, which is beneficial to ensure the crystal precipitation rate in the aging step.

[0046] An embodiment of the present invention also provides a device for the method of concentrating and crystallizing a salt solution as described in the aforementioned embodiment, comprising an evaporator 11, wherein the evaporator 11 is provided with a salt solution inlet and a concentrated salt solution outlet, wherein the concentrated salt solution outlet is sequentially connected to a disperser 7, a thickener 8 and a solid-liquid separation device, and the disperser 7 is provided with a feeding device for adding a dispersant and a common ion acid.

[0047] In an embodiment of the present invention, high-salt wastewater is evaporated and concentrated in an evaporator 11. When the solution in the evaporator 11 begins to precipitate crystals, the solution is transferred to a disperser 7, mixed evenly with a dispersant and a common ion acid, and then transferred to a thickener 8 for aging. After aging, solid-liquid separation is performed to obtain industrial salt with low water content and low impurity content.

[0048] In some embodiments, the evaporator 11 includes a heat exchanger 3 and a separator 4, the salt solution inlet is arranged on the heat exchanger 3, a heat exchange solution outlet is arranged on the top of the heat exchanger 3, the heat exchange solution outlet is connected to the heat exchange solution inlet of the separator 4, the concentrated salt solution outlet is arranged at the bottom of the separator 4, and the concentrated salt solution outlet is respectively connected to the supplementary heat inlet located at the bottom of the heat exchanger 3 and the liquid inlet of the disperser 7;

[0049] The separator 4 is provided with a low-pressure steam outlet at the top, and the heat exchanger 3 is provided with a secondary steam inlet, the low-pressure steam outlet is connected to the secondary steam inlet through a steam pipeline, and the steam pipeline is also connected in series with a spray tower 5 and a compressor 6; the heat exchanger 3 is also connected in front of a preheater 2 for preheating the salt solution;

[0050] The salt leg of the separator 4 is provided with a liquid return inlet, the supernatant outlet of the thickener 8 is connected to the liquid return inlet, and the solid phase outlet of the thickener 8 is connected to the solid-liquid separation device.

[0051] The working process of the salt solution concentration and crystallization device in the embodiment of the present invention is as follows:

[0052] (1) The salt solution is transferred from the stock solution storage tank 1 to the preheater 2 by a pump to exchange heat with the heating steam for preliminary preheating; wherein the preheater 2 can be composed of multiple stages in series as required, and the preheating temperature is 20°C-90°C, specifically 20°C, 40°C, 60°C, 80°C, 90°C or any value between 20°C-90°C, more preferably 80°C-90°C, which is the same as the separation temperature.

[0053] (2) The preheated solution is further heated to the evaporation separation temperature through the heat exchanger 3 and then enters the separator 4.

[0054] (3) The solution is heated in the separator 4 to generate low-pressure steam. Since the low-pressure steam generated by the separator 4 will carry a small amount of foam and solids, the low-pressure steam is transferred to the spray tower 5. After the foam and solids are removed by net spraying, the low-pressure steam is compressed into secondary steam by the compressor 6 to increase the enthalpy and returned to the heat exchanger 3 for use.

[0055] (4) Part of the solution in the separator 4 is returned to the heat exchanger 3 via a forced circulation pump for heating and then continues to return to the separator 4 for separation, and the other part is transferred to the disperser 7 by the liquid transfer pump, wherein the forced circulation pump and the liquid transfer pump are in continuous operation as a whole to avoid crystallization and pipe blockage in the pipeline; the liquid inlet amount of the disperser 7 accounts for 20%-60% of the liquid outlet amount of the concentrated salt solution, specifically, it can be 20%, 30%, 40%, 50%, 60% or any value between 20% and 60%; the remaining part of the concentrated salt solution is continued to return to the separator 4 for separation after heating, which can increase the solute content of the newly-inlet solution in the separator 4 to increase the crystallization rate, and on the other hand, it can provide crystal seeds for the newly-inlet solution;

[0056] (5) Part of the solution in the separator 4 is transferred to the disperser 7 by the liquid transfer pump, and after being mixed with the common ion acid and the dispersant in the disperser 7, it is stirred for a certain period of time to make the components evenly mixed and then transferred to the thickener 8 for aging. The supernatant in the thickener 8 returns to the salt leg part of the separator 4, and the slurry in the lower part of the thickener 8 is transferred to the solid-liquid separation device, such as the centrifuge 9. Normally, the temperature of the disperser 7 is the same as the temperature in the separator 4 or is between the temperatures of the thickener 8 and the separator 4. The supernatant in the thickener 8 returns to the salt leg part of the separator 4. Since crystals are precipitated in the salt leg and small particles of crystals are entrained in the supernatant, the supernatant returning to the salt leg can provide seeds for the precipitated crystals and increase the crystallization rate.

[0057] (6) The solid obtained by the solid-liquid separation device is industrial salt, and the centrifuged mother liquor can be transferred to the mother liquor storage tank 10, and the lithium therein is subsequently recovered.

[0058] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0059] Example 1

[0060] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, wherein the device used is as follows: Figure 1 As shown, the following specific steps are included:

[0061] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1:

[0062] Table 1

[0063]

[0064] The salt solution is transferred from the stock liquid storage tank 1 to the preheater 2 for steam heating through a pump, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3. The heat exchanger 3 is a forced circulation heat exchanger to maintain the solution at 80°C. The heated solution enters the separator 4 to maintain a temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is compressed into secondary steam by the compressor 6 after removing the entrained foam and materials by the spray tower 5, and returned to the heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump and continues to evaporate; the remaining 40% is transferred to the disperser 7 by the liquid transfer pump, and polyethylene glycol and sulfuric acid are added to the mass fraction of both 5%. After mixing evenly, the solution is transferred to the thickener 8 to cool to 60°C and aged at 60°C for 0.5h. The supernatant in the thickener 8 returns to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0065] Embodiment 2:

[0066] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, comprising the following specific steps:

[0067] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1;

[0068] The salt solution is transferred from the stock liquid storage tank 1 to the preheater 2 for steam heating through a pump, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3. The heat exchanger 3 is a forced circulation heat exchanger to maintain the solution at 80°C. The heated solution enters the separator 4 to maintain a temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is compressed into secondary steam by the compressor 6 after removing the entrained foam and materials by the spray tower 5, and returned to the heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump and continues to evaporate; the remaining 40% is transferred to the disperser 7 by the liquid transfer pump, and polyethylene glycol and sulfuric acid are added to the mass fraction of both to 10%. After mixing evenly, it is transferred to the thickener 8 for aging at 60°C for 1h, and the supernatant in the thickener 8 returns to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0069] Embodiment 3:

[0070] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, comprising the following specific steps:

[0071] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1; the salt solution is transferred from the stock solution storage tank 1 to the preheater 2 for steam heating through a pump, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3, which is a forced circulation heat exchanger to maintain the solution at 80°C. The heated solution enters the separator 4 to maintain the temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is compressed into secondary steam by the compressor 6 after the entrained foam and materials are removed by the spray tower 5, and returned to the heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump and continues to evaporate; the remaining 40% is transferred to the disperser 7 by the liquid transfer pump, and polyethylene glycol and sulfuric acid are added until the mass fraction of both is 20%. After mixing evenly, it is transferred to the thickener 8 for aging at 60°C for 2h, the supernatant in the thickener 8 is returned to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0072] Example 4

[0073] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, which differs from the embodiment 3 only in that the amount of polyethylene glycol added is increased to 30%. However, adding excessive dispersant will make crystal growth difficult, resulting in small crystal particles, which cannot meet the expected particle size and water content requirements.

[0074] Example 5

[0075] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, which is different from the embodiment 3 only in that the amount of sulfuric acid added is increased to 30%. Excessive acid will make the solution viscous, resulting in ineffective separation of water during solid-liquid separation, and the solid water content is high.

[0076] Example 6

[0077] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater. The only difference from Example 3 is that the dispersant is replaced by polyvinyl alcohol. Since the hydroxyl group forms hydrogen bonds with water, the viscosity of the liquid increases, resulting in a higher water content of the obtained solid during solid-liquid separation.

[0078] Example 7

[0079] This embodiment provides a method for concentrating and crystallizing high-salt wastewater, which is different from Embodiment 3 only in that the salt solution is the raffinate, and the composition is shown in Table 2.

[0080] Table 2

[0081]

[0082] Example 8

[0083] This embodiment provides a method for concentrating and crystallizing high-salt wastewater. The only difference from Embodiment 3 is that 40% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating and continued evaporation under the action of a forced circulation pump; the remaining 60% is transferred to the disperser 7 by a liquid transfer pump.

[0084] Example 9

[0085] This embodiment provides a method for concentrating and crystallizing high-salt wastewater. The only difference from Example 3 is that 80% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating and continued evaporation under the action of a forced circulation pump; the remaining 20% ​​is transferred to the disperser 7 by a liquid transfer pump.

[0086] Comparative Example 1:

[0087] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, comprising the following specific steps:

[0088] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1;

[0089] The salt solution is transferred from the stock liquid storage tank 1 to the preheater 2 for steam heating through a pump, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3. The heat exchanger 3 is a forced circulation heat exchanger to maintain the solution at 80°C. The heated solution enters the separator 4 to maintain a temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is compressed into secondary steam by the compressor 6 after removing the entrained foam and materials by the spray tower 5, and returned to the forced circulation heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump and continues to evaporate; the remaining 40% is transferred to the disperser 7 by the liquid transfer pump, and sulfuric acid is added to a mass fraction of 20%. After mixing evenly, it is transferred to the thickener 8 for aging at 60°C for 2h, and the supernatant in the thickener 8 returns to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0090] Comparative Example 2:

[0091] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, comprising the following specific steps:

[0092] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1;

[0093] The salt solution is transferred from the stock liquid storage tank 1 to the preheater 2 for steam heating through a pump, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3. The heat exchanger 3 is a forced circulation heat exchanger to maintain the solution at 80°C. The heated solution enters the separator 4 to maintain a temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is compressed into secondary steam by the compressor 6 after removing the entrained foam and materials by the spray tower 5, and returned to the heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump and continues to evaporate; the remaining 40% is transferred to the disperser 7 by the liquid transfer pump, and polyethylene glycol is added to a mass fraction of 20%. After mixing evenly, it is transferred to the thickener 8 for aging at 60°C for 2h, and the supernatant in the thickener 8 returns to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0094] Comparative Example 3:

[0095] This embodiment provides a method for concentrating and crystallizing lithium extraction wastewater, comprising the following specific steps:

[0096] The sulfate system lithium precipitation mother liquor is decarbonized and adjusted, and the composition of the obtained salt solution is shown in Table 1;

[0097] The salt solution is transferred from the stock solution storage tank 1 to the preheater 2 through a pump for steam heating, preheated to 80-90°C, and then supplemented with heat in the heat exchanger 3. The heat exchanger 3 is a forced circulation heat exchanger that maintains the solution at 80°C. The heated solution enters the separator 4 to maintain a temperature not lower than 80°C and precipitate crystals to generate low-pressure steam. The low-pressure steam is removed from the entrained foam and materials by the spray tower 5 and compressed into secondary steam by the compressor 6. It is returned to the heat exchanger 3 for use to enhance heat recovery. 60% of the volume of the solution in the separator is transferred to the heat exchanger 3 for heating under the action of the forced circulation pump, and evaporation continues. The remaining 40% is transferred by the liquid transfer pump to the thickener 8 for aging at 60°C for 2 hours. , The supernatant in the thickener 8 is returned to the salt leg of the separator 4, and the slurry in the thickener 8 is transferred to the centrifuge 9 for solid-liquid separation to obtain the target solid and mother liquor.

[0098] The purity, moisture content, lithium content, proportion of particles smaller than 60 mesh, and lithium loss of the sodium sulfate solid obtained after continuous operation of the above embodiments and comparative examples are shown in Table 3.

[0099] Table 3

[0100]

[0101] Different from Example 3, in Comparative Example 1, polyethylene glycol was not added, and the obtained solid was severely agglomerated. Due to the agglomeration and entrainment, the lithium loss increased and the purity of the industrial salt decreased.

[0102] Different from Example 3, in Comparative Example 2, sulfuric acid is not added, and the thickening process relies solely on physical thickening, resulting in a small particle size of the obtained solid particles, a reduced purity, and an increased water content and lithium entrainment loss.

[0103] Different from Example 3, Comparative Example 3 does not add a disperser 7 before the thickener 8, and does not add polyethylene glycol and sulfuric acid. The thickener 8 is directly used for aging, and the obtained solid particles have a small particle size, reduced purity, and significantly increased water content and lithium entrainment loss.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for concentrating and crystallizing a salt solution, characterized in that: include: Concentrating the salt solution to obtain a concentrated salt solution, mixing the concentrated salt solution with a dispersant and a common ion acid to obtain a mixed solution; aging and solid-liquid separation of the mixed solution to obtain industrial salt; Wherein, the common ion acid is an acid having the same anion as the industrial salt.

2. The method for concentrating and crystallizing a salt solution according to claim 1, characterized in that: The mass fraction of the dispersant in the mixed liquid is 5wt%-20wt%; And / or, the dispersant is an alcohol or a ketone.

3. The method for concentrating and crystallizing a salt solution according to claim 1, characterized in that: The mass fraction of the common ion acid in the mixed solution is 5wt%-20wt%; And / or, 20% to 60% of the volume of the concentrated salt solution is mixed with a dispersant and a common ion acid to obtain a mixed solution, and the remaining concentrated salt solution is mixed with the salt solution and then concentrated again.

4. The method for concentrating and crystallizing a salt solution according to claim 1, characterized in that: The aging is carried out in a thickener, the aging time is 0.5h-2h, and the aging temperature is 50°C-80°C; And / or, the concentration temperature is 80°C-90°C.

5. The method for concentrating and crystallizing a salt solution according to claim 1, characterized in that: The salt solution is at least one of a lithium precipitation mother liquor, a raffinate produced in a lithium extraction process, and a high-boron solution produced in a lithium extraction process from a salt lake; And / or, the concentrated salt solution is a saturated solution of the industrial salt.

6. A device for use in the method for concentrating and crystallizing a salt solution according to claim 1, characterized in that: The invention comprises an evaporator, wherein the evaporator is provided with a salt solution inlet and a concentrated salt solution outlet, wherein the concentrated salt solution outlet is sequentially connected with a disperser, a thickener and a solid-liquid separation device, and the disperser is provided with a feeding device for adding a dispersant and a common ion acid.

7. The device according to claim 6, characterized in that The evaporator includes a heat exchanger and a separator, the salt solution inlet is arranged on the heat exchanger, a heat exchange solution outlet is arranged on the top of the heat exchanger, the heat exchange solution outlet is connected to the heat exchange solution inlet of the separator, the concentrated salt solution outlet is arranged at the bottom of the separator, and the concentrated salt solution outlet is respectively connected to the heat supplement inlet located at the bottom of the heat exchanger and the liquid inlet of the disperser.

8. The device according to claim 7, characterized in that The salt leg of the separator is provided with a liquid return inlet, the supernatant outlet of the thickener is connected to the liquid return inlet, and the solid phase outlet of the thickener is connected to the solid-liquid separation device.

9. The device according to claim 7, characterized in that A low-pressure steam outlet is provided on the top of the separator, a secondary steam inlet is provided on the heat exchanger, the low-pressure steam outlet is connected to the secondary steam inlet through a steam pipeline, and a spray tower and a compressor are also connected in series on the steam pipeline.

10. The device according to claim 7, characterized in that A preheater for preheating the salt solution is also connected in front of the heat exchanger.

Citation Information

Patent Citations

  • Garbage fly ash water washing liquid evaporation desalination system and method

    CN105016555A

  • Potassium perchlorate effluent brine treatment apparatus, and technology for recovering potassium perchlorate and sodium chloride from potassium perchlorate effluent brine

    CN106007135A

  • MVR evaporative concentration and crystallization process for extracting lithium from salt lake brine

    CN107308662A

  • Method for preparing anti-hard agglomerated nano alumina particles

    CN109534378A