Nano-filtration membrane with organic pollution resistance and antibacterial property and preparation method of nano-filtration membrane

By forming an anti-organic pollution antibacterial ultra-thin layer with covalent bonding on the nanofiltration membrane, the anti-pollution and antibacterial ability of the membrane surface is enhanced by using polyvinyl alcohol and metal ions to enhance the anti-pollution and antibacterial ability of the nanofiltration membrane in actual applications, the organic pollution and microbial pollution in practical applications are solved. The problem of this has achieved long-term stable and efficient operation.

CN118925521AInactive Publication Date: 2024-11-12TIANJIN SEA WATER DESALINATION & COMPLEX UTILIZATION INST STATE OCEANOGRAPHI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411293762.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In actual applications, existing nanofiltration membranes are susceptible to organic contamination and microbial contamination, resulting in a decline in membrane performance. Most existing methods only focus on anti-one type of pollution, and organic pollutants can become nutrients for bacteria to promote bacterial growth. Affects the long-term and stable operation of the membrane.

Method used

The porous ultrafiltration membrane support layer is used to impregnate polyamine and polyacid chloride in turn to form a polyamide separation layer, and immerse it in the anti-organic pollution anti-bacterial ultra-thin layer preparation solution to form an anti-organic pollution anti-bacterial ultra-thin layer with covalent bonding. The formation of hydrophilic layers and metal ions through polyvinyl alcohol imparts antibacterial properties, enhancing the anti-pollution and antibacterial ability of the membrane surface.

Benefits of technology

The nanofiltration membrane has been maintained for a long time with anti-organic pollution and antibacterial properties, reduced organic matter adsorption and bacterial proliferation, improved the stability and service life of the membrane, and is suitable for water resource development and wastewater recycling and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925521A_ABST
    Figure CN118925521A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a nanofiltration membrane with both organic pollution resistance and antibacterial property and a preparation method thereof, and the preparation method comprises the following steps: sequentially dipping a porous ultrafiltration membrane support layer in a water phase solution containing polyamine and an organic phase solution containing polyacyl chloride, carrying out interfacial polymerization reaction on the polyamine and the polyacyl chloride to generate a polyamide separation layer of the nanofiltration membrane; the polyamide separation layer is soaked in an anti-organic-pollution antibacterial ultrathin layer preparation solution to form an anti-organic-pollution antibacterial ultrathin layer, and the porous ultrafiltration membrane supporting layer, the polyamide separation layer and the anti-organic-pollution antibacterial ultrathin layer serve as the composite nanofiltration membrane with the anti-organic-pollution and antibacterial properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nanofiltration membrane preparation, and in particular to a nanofiltration membrane with both organic pollution resistance and antibacterial properties and a preparation method thereof. Background Art

[0002] As a mainstream nanofiltration membrane product, polyamide composite nanofiltration membrane has been widely used in water resource development and wastewater recycling due to its good separation ability. However, in actual application, due to the hydrophobicity and charge characteristics of the polyamide material on the surface of the nanofiltration membrane, organic pollutants and bacteria are very easy to deposit and adhere on the membrane surface, resulting in a sharp decline in membrane performance. Physical or chemical cleaning of the membrane surface is a common method to reduce pollution, but frequent cleaning not only increases the system operating cost, but also destroys the separation performance of the membrane, resulting in a reduction in service life. Therefore, improving the anti-organic pollution and antibacterial properties of the nanofiltration membrane surface has important theoretical and application value to ensure the long-term stable operation of the nanofiltration membrane system.

[0003] The pollution types of nanofiltration membrane mainly include inorganic pollution, organic pollution and microbial pollution. Organic pollution and microbial pollution are common and influential pollution types in the actual use of nanofiltration membrane, which pose a great threat to membrane performance and service life. In response to these pollutions, the commonly used methods are to use new reaction monomers, membrane surface coating and grafting. For example, the method of adding polyvinyl alcohol to an aqueous solution to prepare an anti-pollution nanofiltration membrane, but because polyvinyl alcohol is a polymer, it is not easy to diffuse to the membrane surface during interfacial polymerization, resulting in its distribution on the membrane surface being limited, affecting the performance of anti-pollution. For another example, the method of using antibacterial metal ions on the surface of a polyamide composite nanofiltration membrane can obtain an antibacterial nanofiltration membrane, but the antibacterial metal ions are loaded on the membrane surface through physical action. During the use of the membrane, due to hydraulic scouring, there is a problem of loss of antibacterial metal ions. The method of coating a polyvinyl alcohol functional layer on the membrane surface is used to regulate the charge of the membrane surface and inhibit the adsorption of pollutants, but polyvinyl alcohol has no antibacterial properties. Since bacteria have a strong proliferation ability, even if only a small amount is attached to the membrane surface, they will proliferate rapidly, causing membrane pollution and performance degradation.

[0004] Although the prior art provides some methods to improve the anti-fouling or antibacterial properties of membranes, these methods still have some weaknesses, and most methods only focus on one aspect of anti-organic pollution or antibacterial performance. In actual membrane applications, these two types of pollution often exist at the same time, and organic pollutants on the membrane surface can also become nutrients for bacteria, providing favorable conditions for the growth and reproduction of bacteria. Therefore, the development of nanofiltration membranes that are both anti-organic pollution and antibacterial can synergistically promote the long-term stable and efficient operation of the membrane. Summary of the invention

[0005] The embodiments of this specification provide a nanofiltration membrane with both resistance to organic pollution and antibacterial properties and a preparation method thereof, which are used to solve the following technical problems: Although the prior art provides some methods to improve the anti-pollution or antibacterial properties of the membrane, these methods still have some weaknesses, and most methods only focus on one aspect of the anti-organic pollution or antibacterial properties. In the actual application of the membrane, these two types of pollution often exist at the same time, and the organic pollutants on the membrane surface can also become nutrients for bacteria, providing favorable conditions for the growth and reproduction of bacteria.

[0006] To solve the above technical problems, the embodiments of this specification are implemented as follows: The present invention provides a method for preparing a nanofiltration membrane having both anti-organic pollution and antibacterial properties, comprising: The porous ultrafiltration membrane support layer is sequentially immersed in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride, so that the polyamine and the polyacyl chloride undergo an interfacial polymerization reaction to form a polyamide separation layer of the nanofiltration membrane; The polyamide separation layer is immersed in an anti-organic pollution antibacterial ultra-thin layer preparation solution to form an anti-organic pollution antibacterial ultra-thin layer. The porous ultrafiltration membrane support layer, the polyamide separation layer and the anti-organic pollution antibacterial ultra-thin layer serve as a composite nanofiltration membrane with both anti-organic pollution and antibacterial properties.

[0007] The present specification provides a nanofiltration membrane with both organic pollution resistance and antibacterial properties. The composite nanofiltration membrane is prepared by the preparation method described in the claims. The composite nanofiltration membrane comprises: Porous ultrafiltration membrane support layer, polyamide separation layer and anti-organic pollution and antibacterial ultra-thin layer; in, The porous ultrafiltration membrane support layer is located at the bottom of the composite nanofiltration membrane, and the porous ultrafiltration membrane support layer is a polysulfone ultrafiltration membrane and / or a polyethersulfone ultrafiltration membrane; The polyamide separation layer is located in the middle of the composite nanofiltration membrane, and the polyamide separation layer covers the porous ultrafiltration membrane support layer; The anti-organic pollution and antibacterial ultra-thin layer is located on the top of the composite nanofiltration membrane, and is bonded to the polyamide separation layer through a covalent bond and attached to the polyamide separation layer. The anti-organic pollution and antibacterial ultra-thin layer is composed of a polymer main material, a chelating agent and antibacterial metal ions, and the polymer main material is connected to the chelating agent through a covalent bond, and the chelating agent is bonded to the antibacterial metal ions through a coordination bond.

[0008] The embodiments of this specification provide a nanofiltration membrane with both resistance to organic pollution and antibacterial properties and a preparation method thereof. The method comprises the following steps: the porous ultrafiltration membrane support layer is sequentially immersed in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride, so that the polyamine and the polyacyl chloride undergo an interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane; the polyamide separation layer is immersed in an anti-organic pollution antibacterial ultrathin layer preparation solution to form an anti-organic pollution antibacterial ultrathin layer. The porous ultrafiltration membrane support layer, the polyamide separation layer and the anti-organic pollution antibacterial ultrathin layer serve as a composite nanofiltration membrane with both resistance to organic pollution and antibacterial properties. A ternary component is used to construct an anti-organic pollution antibacterial ultrathin layer to modify the surface of the nanofiltration membrane. The polymer main material polyvinyl alcohol forms a hydrophilic layer on the membrane surface. The polyhydroxy structure enhances the combination of the membrane surface with water molecules to prevent the adsorption and deposition of organic matter on the membrane surface. At the same time, polyvinyl alcohol and the polyamide separation layer are covalently bonded, and the strong chemical bond makes the interaction between the anti-organic pollution antibacterial ultra-thin layer and the separation layer stronger, thereby enhancing the stability of the anti-organic pollution antibacterial ultra-thin layer during use. Metal ions give the membrane surface antibacterial properties, inactivate bacteria close to the membrane surface, and prevent bacteria from proliferating on the membrane surface. Chelating agents connect polyvinyl alcohol and metal ions, increase the metal ion loading on the membrane surface, and enhance the stability of the anti-pollution layer. The preparation method of the nanofiltration membrane with both anti-organic pollution and antibacterial properties is simple and easy to industrialize. The resulting nanofiltration membrane can maintain good anti-organic pollution and antibacterial properties for a long time, and can be used in fields such as water resource development and wastewater recycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 A schematic diagram of a method for preparing a nanofiltration membrane having both organic pollution resistance and antibacterial properties provided in an embodiment of this specification. DETAILED DESCRIPTION

[0010] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0011] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0012] Materials used in the present invention: There is no particular limitation on the sources of all raw materials in the present invention and the following embodiments and comparative examples, and any raw materials may be commercially available.

[0013] Figure 1 Schematic diagram of the method for preparing a nanofiltration membrane with both organic pollution resistance and antibacterial properties provided in the embodiments of this specification. Figure 1 As shown, the preparation method comprises: Step 101: immersing the porous ultrafiltration membrane support layer in an aqueous solution containing polyamine and an organic solution containing polyacyl chloride in sequence, so that the polyamine and the polyacyl chloride undergo interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane.

[0014] In the embodiment of the present specification, the polyamine-containing solution is piperazine, and the composition of the aqueous phase solution containing the polyamine includes: an aqueous solution of 0.5-5.0 wt% of piperazine, 0.3-2.0 wt% of triethylamine, and 0.01-0.5 wt% of sodium dodecyl sulfate; The polyacyl chloride is trimesoyl chloride, and the composition of the organic phase solution containing the polyacyl chloride includes: an Isopar G solution containing 0.05-0.5 wt % of trimesoyl chloride.

[0015] In the embodiment of the present specification, the porous ultrafiltration membrane support layer is a polysulfone ultrafiltration membrane, and the pore size distribution of the porous ultrafiltration membrane support layer is 30 nm - 100 nm.

[0016] It should be noted that in the embodiments of this specification, the pore size distribution of the porous ultrafiltration membrane support layer can be uniform or inconsistent, and whether the pore size is uniform does not limit the manufacturing method of the present application. In a specific embodiment, the pore size distribution of the porous ultrafiltration membrane support layer is preferably 30 nm-50 nm.

[0017] In the embodiment of the present specification, the porous ultrafiltration membrane support layer is sequentially immersed in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride, so that the polyamine and the polyacyl chloride undergo an interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane, specifically comprising: After the porous ultrafiltration membrane support layer is contacted with the aqueous phase solution containing the polyamine according to a first contact condition, the porous ultrafiltration membrane support layer is contacted with the organic phase solution containing the polyacid chloride according to a second contact condition, and heat-treated according to a heat treatment condition, so that the polyamine and the polyacid chloride undergo an interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane; in, The first contact condition is: contact time is 20-120s, contact temperature is 15-30°C; The second contact condition is: contact time is 20-120s, contact temperature is 15-30°C; The heat treatment conditions are: treatment temperature is 40-80°C, and treatment time is 2-10min.

[0018] The purpose of the interfacial polymerization reaction between the polyamine and the polyacyl chloride by sequentially immersing in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride is to obtain a polyamide separation layer of the nanofiltration membrane. In this embodiment of the present application, the first contact condition is preferably 25°C, 60 s, the second contact condition is preferably 25°C, 60 s, and the heat treatment condition is preferably 50°C, 5 min.

[0019] Step 103: Immersing the polyamide separation layer in an anti-organic pollution antibacterial ultra-thin layer preparation solution to form an anti-organic pollution antibacterial ultra-thin layer, the porous ultrafiltration membrane support layer, the polyamide separation layer and the anti-organic pollution antibacterial ultra-thin layer serve as a composite nanofiltration membrane with both anti-organic pollution and antibacterial properties.

[0020] In the embodiment of the present specification, the solution for preparing the anti-organic pollution antibacterial ultra-thin layer comprises a polymer main material, a chelating agent and a metal ion, wherein the polymer main material is a polyhydroxy polymer, the chelating agent is an amino polyacid, and the metal ion is a copper ion or a silver ion. The preparation process of the solution for preparing the anti-organic pollution antibacterial ultra-thin layer comprises: Dissolving the chelating agent in deionized water, adjusting the pH to 8.5, and adding the chelating agent to the soluble inorganic salt solution of the metal ion to generate a metal chelate solution; The metal chelate solution is added into the aqueous solution of the polymer main material, and the pH is adjusted to a preset pH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer.

[0021] In the examples of this specification, the polyhydroxy polymer is polyvinyl alcohol, and the concentration of the polyvinyl alcohol is 5-15 g / L; The amino polyacid is any one of ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, and triethylenetetraaminehexaacetic acid, and the concentration of the chelating agent is 5-15 mM; The concentration of the soluble inorganic salt in the soluble inorganic salt solution of metal ions is 5-15 mM.

[0022] In the embodiments of the present specification, the soluble inorganic salt solution of metal ions is AgNO3 or CuSO4.

[0023] In the examples of this specification, the preset pH is 8.0-9.0; The step of adding the metal chelate solution to the aqueous solution of the polymer main material and adjusting the pH to a preset pH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer specifically includes: The metal chelate solution is added into the aqueous solution of the polymer main material, and the pH is adjusted to 8.0-9.0 with NaOH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer.

[0024] In the embodiment of the present specification, the polyamide separation layer is immersed in the solution for preparing the anti-organic pollution antibacterial ultra-thin layer to form the anti-organic pollution antibacterial ultra-thin layer, which specifically includes: The polyamide separation layer is immersed in the anti-organic pollution antibacterial thin layer preparation solution according to the third contact condition, and is dried to form the anti-organic pollution antibacterial ultra-thin layer.

[0025] In the examples of this specification, the third contact condition is: contact time is 1-10 min, temperature is 25-35°C; The drying treatment adopts oven drying, and the oven drying conditions are: 60-100°C, 3-10min.

[0026] The present invention provides a nanofiltration membrane having both anti-organic pollution and antibacterial properties, including: Porous ultrafiltration membrane support layer, polyamide separation layer and anti-organic pollution and antibacterial ultra-thin layer; in, The porous ultrafiltration membrane support layer is located at the bottom of the composite nanofiltration membrane, and the porous ultrafiltration membrane support layer is a polysulfone ultrafiltration membrane and / or a polyethersulfone ultrafiltration membrane; The polyamide separation layer is located in the middle of the composite nanofiltration membrane, and the polyamide separation layer covers the porous ultrafiltration membrane support layer; The anti-organic pollution and antibacterial ultra-thin layer is located on the top of the composite nanofiltration membrane, and is bonded to the polyamide separation layer through a covalent bond and attached to the polyamide separation layer. The anti-organic pollution and antibacterial ultra-thin layer is composed of a polymer main material, a chelating agent and antibacterial metal ions, and the polymer main material is connected to the chelating agent through a covalent bond, and the chelating agent is bonded to the antibacterial metal ions through a coordination bond.

[0027] The nanofiltration membrane provided in the embodiments of this specification, which has both resistance to organic pollution and antibacterial properties, can be applied to water treatment nanofiltration membranes and components.

[0028] In order to further understand the method provided in this embodiment, the method used or may be used in the embodiments or comparative examples of the present invention is described below: 1. Evaluation of anti-organic pollution performance The protein pollution test was used to calculate the flux attenuation rate and flux recovery rate of the membrane to characterize the anti-organic pollution performance of the nanofiltration membrane. The main steps were: using a cross-flow membrane detection device, the NaCl concentration on the raw material side was 2000 ppm, the operating pressure was 0.69 MPa, and the pre-pressure was 0.5 h. Bovine serum albumin was added to the raw material, and the concentration of bovine serum albumin was 300 ppm. The water flux of the nanofiltration membrane was recorded when the protein pollution began. J0. The membrane was run for another 10 h, and the water flux of the nanofiltration membrane was recorded at the end of protein contamination. J 1. Replace the raw material solution with pure water and rinse the surface of the nanofiltration membrane for 30 min. Use a mixed aqueous solution of 2000 ppm sodium chloride and 300 ppm bovine serum albumin as the influent raw material solution again, test the membrane at 0.69 MPa, and record the water flux of the membrane. J 2.

[0029] Flux decay rate of the membrane ( FDR ): FDR =( J 0- J 1) / J 0×100% Flux recovery rate ( FRR ): FRR = J 2 / J 0×100% 2. Evaluation of antibacterial properties The antibacterial properties of the nanofiltration membrane were characterized by a bactericidal test. The main steps were as follows: Escherichia coli was incubated in a culture medium, cultured overnight in a 37°C constant temperature shaker until the bacteria reached the logarithmic growth phase, and diluted with physiological saline to a bacterial concentration of about 1.0×10 6 CFU / mL suspension. The non-woven fabric side of the nanofiltration membrane was attached to a glass slide, and the anti-organic pollution antibacterial ultra-thin layer was exposed, with a size of 2.6×7.6 cm. 60 μL of bacterial suspension was evenly coated on the membrane surface and covered with a glass slide to ensure that the bacterial liquid was evenly dispersed and not easily volatile. The membrane and the glass slide were placed in a sterile culture dish together, incubated in a 37°C constant temperature incubator for 3 hours, and then the membrane surface and the glass slide in contact with the membrane surface were washed with 9 mL of physiological saline to collect bacteria. 1 mL of it was evenly mixed with the culture medium; it was placed in a 37°C constant temperature incubator for 48 hours, the colonies were counted, and the antibacterial activity was calculated.

[0030] In the embodiments of this specification, the calculation of antibacterial property is realized by antibacterial rate. R The calculation is: R =( B - A ) / B ×100%, where B is the number of viable bacteria on the culture medium corresponding to the comparative nanofiltration membrane, A is the number of viable bacteria on the culture medium corresponding to the nanofiltration membrane of the embodiment.

[0031] Comparative Example 1 A nanofiltration membrane without an ultra-thin layer of organic pollution resistance and antibacterial properties is used as comparative example 1, and its preparation method is as follows: preparing an aqueous solution with a piperazine content of 1.5 wt%, a triethylamine content of 1.0 wt% and a sodium dodecyl sulfate content of 0.1 wt%; preparing an Isopar G organic solution with a trimesoyl chloride content of 0.1 wt%; soaking a porous ultrafiltration support membrane with deionized water, and blowing nitrogen gas on the membrane surface until there are no droplets; immersing the surface of the porous ultrafiltration support membrane in the aqueous solution, contacting for 60 s, and blowing nitrogen gas on the membrane surface until there are no droplets; immersing the surface of the support membrane containing an aqueous phase monomer in an organic phase solution, contacting for 60 s, to obtain a nanofiltration membrane; placing the nanofiltration membrane in an oven at 50°C for heat treatment for 5 min to further crosslink the separation layer polyamide; washing the surface with deionized water, and storing it in deionized water for standby use.

[0032] The nanofiltration membrane obtained in Comparative Example 1 was evaluated for its anti-organic pollution performance and antibacterial performance. The evaluation details are shown in Table 1. Example 1

[0033] A nanofiltration membrane having only polyvinyl alcohol in the ultra-thin layer is used as comparative example 2, and its preparation method is as follows: prepare a nanofiltration membrane by the method of comparative example 1; dissolve polyvinyl alcohol in deionized water at a concentration of 10 g / L, stir it at 90°C to dissolve it, and let it stand to cool; immerse the surface of the nanofiltration membrane in the polyvinyl alcohol solution, contact it at 25°C for 2 min, remove excess solution, and treat it in an oven at 80°C for 10 min; wash the surface with deionized water, and store it in deionized water for use.

[0034] The nanofiltration membrane obtained in Example 1 was evaluated for its anti-organic pollution performance and antibacterial performance. The evaluation results are shown in Table 1. Example 2

[0035] A nanofiltration membrane having only polyvinyl alcohol and diethylenetriaminepentaacetic acid in an ultra-thin layer is used as comparative example 2, and its preparation method is as follows: prepare a nanofiltration membrane according to the method of comparative example 1; dissolve polyvinyl alcohol in deionized water, stir it at 90°C to dissolve it, and let it stand to cool; dissolve diethylenetriaminepentaacetic acid in deionized water and stir it thoroughly; pour the diethylenetriaminepentaacetic acid solution into the polyvinyl alcohol solution to make the concentration of polyvinyl alcohol in the final solution be 10 g / L and the concentration of diethylenetriaminepentaacetic acid be 10 mM; immerse the surface of the nanofiltration membrane in the solution, contact it at 25°C for 2 min, remove excess solution, and treat it in an oven at 80°C for 5 min; wash the surface with deionized water, and store it in deionized water for use.

[0036] The anti-organic pollution performance and antibacterial performance of the nanofiltration membrane obtained in Example 2 were evaluated. The evaluation results are shown in Table 1. Example 3

[0037] A nanofiltration membrane containing polyvinyl alcohol, diethylenetriamine pentaacetic acid and copper ions in an ultra-thin layer is used as comparative example 1, and its preparation method is as follows: prepare a nanofiltration membrane according to the method of comparative example 1; dissolve polyvinyl alcohol in deionized water, stir it at 90°C to dissolve it, and let it stand to cool; dissolve diethylenetriamine pentaacetic acid in deionized water, add CuSO4, and stir it thoroughly; pour the mixed solution of diethylenetriamine pentaacetic acid and CuSO4 into the polyvinyl alcohol solution to make the concentration of polyvinyl alcohol in the final solution be 10 g / L, the concentration of diethylenetriamine pentaacetic acid be 10 mM, and the concentration of CuSO4 be 10 mM; immerse the surface of the nanofiltration membrane in the solution, contact it at 25°C for 2 min, remove excess solution, and treat it in an oven at 80°C for 5 min; wash the surface with deionized water, and store it in deionized water for use.

[0038] The nanofiltration membrane obtained in Example 3 was evaluated for its anti-organic pollution performance and antibacterial performance. The evaluation results are shown in Table 1. Example 4

[0039] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 was poured into the polyvinyl alcohol solution to make the final solution have a polyvinyl alcohol concentration of 10 g / L, a diethylenetriaminepentaacetic acid concentration of 10 mM, and an AgNO3 concentration of 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 2 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water and stored in deionized water for later use.

[0040] The nanofiltration membrane obtained in Example 4 was evaluated for its anti-organic pollution performance and antibacterial performance. The evaluation results are shown in Table 1.

[0041] Table 1. Data table of anti-organic pollution and antibacterial performance of composite nanofiltration membrane

[0042] From the experimental results in Table 1, it can be seen that, relative to Comparative Example 1, the flux attenuation rate of Examples 1-4 after pollution is significantly reduced, and the flux recovery rate after cleaning is significantly improved, indicating that the construction of the anti-organic pollution antibacterial ultra-thin layer can reduce the binding force between the membrane surface and organic pollutants, prevent organic matter from being adsorbed and accumulated on the membrane surface, and improve the anti-organic pollution performance of the nanofiltration membrane. Compared with Comparative Example 1, the antibacterial rate of Examples 3 and 4 is significantly improved. Copper ions and silver ions are introduced into the anti-pollution antibacterial ultra-thin layers of Examples 3 and 4, respectively, which can kill more than 99% of the bacteria falling on the membrane surface, prevent bacteria from proliferating on the membrane surface, and improve the antibacterial performance of the nanofiltration membrane.

[0043] Taking the results in Table 1 into consideration, when polyvinyl alcohol, chelating agents and antibacterial metal ions are used to construct an ultra-thin layer that resists organic pollution and antibacterial properties, a nanofiltration membrane with both anti-organic pollution and antibacterial properties can be obtained.

[0044] In addition, in order to further verify the preparation method of the nanofiltration membrane having both anti-organic pollution and antibacterial properties in the examples of this specification, the preparation method was verified as follows. Example 5

[0045] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 30°C for 2 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use. Example 6

[0046] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 35°C for 2 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use. Example 7

[0047] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 3 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use. Example 8

[0048] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into the polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 4 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water and stored in deionized water for later use. Example 9

[0049] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 5 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use. Example 10

[0050] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 7 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use. Embodiment 11

[0051] A nanofiltration membrane was prepared by the method of Comparative Example 1; polyvinyl alcohol was dissolved in deionized water, stirred at 90°C to dissolve it, and allowed to stand to cool; diethylenetriaminepentaacetic acid was dissolved in deionized water, AgNO3 / CuSO4 was added, and the mixture was stirred thoroughly; a mixed solution of diethylenetriaminepentaacetic acid and AgNO3 / CuSO4 was poured into a polyvinyl alcohol solution, so that the concentration of polyvinyl alcohol in the final solution was 10 g / L, the concentration of diethylenetriaminepentaacetic acid was 10 mM, and the concentration of AgNO3 / CuSO4 was 10 mM; the surface of the nanofiltration membrane was immersed in the solution, contacted at 25°C for 10 min, excess solution was removed, and the membrane was treated in an oven at 80°C for 5 min; the surface was washed with deionized water, and the membrane was stored in deionized water for later use.

[0052] The nanofiltration membranes obtained in Examples 5-11 were evaluated for their anti-organic pollution performance and antibacterial performance. The evaluation results are shown in Table 2.

[0053] Table 2. Data table of anti-organic pollution and antibacterial performance of composite nanofiltration membrane

[0054] Taking the results of Table 2 into consideration, the method for preparing a nanofiltration membrane with both anti-organic pollution and antibacterial properties provided in this specification is adopted, and the contact time of the third contact condition is 2-10 min, and the contact time of the third contact condition is preferably 2-5 min. At the same time, the contact temperature of the third contact condition has no obvious effect on the preparation method of the present application.

[0055] The above is only a preferred embodiment of the present invention, and is not intended to limit the embodiment. It should be noted that, for those skilled in the art, other different forms of changes or modifications can be made without departing from the principles of the present invention, and the obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing a composite nanofiltration membrane having both anti-organic pollution and antibacterial properties, It is characterized in that The preparation method comprises: The porous ultrafiltration membrane support layer is sequentially immersed in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride, so that the polyamine and the polyacyl chloride undergo an interfacial polymerization reaction to form a polyamide separation layer of the nanofiltration membrane; The polyamide separation layer is immersed in an anti-organic pollution antibacterial ultra-thin layer preparation solution to form an anti-organic pollution antibacterial ultra-thin layer. The porous ultrafiltration membrane support layer, the polyamide separation layer and the anti-organic pollution antibacterial ultra-thin layer serve as a composite nanofiltration membrane with both anti-organic pollution and antibacterial properties.

2. The preparation method according to claim 1, It is characterized in that The polyamine is piperazine, and the aqueous phase solution containing the polyamine comprises: an aqueous solution of 0.5-5.0 wt% piperazine, 0.3-2.0 wt% triethylamine, and 0.01-0.5 wt% sodium dodecyl sulfate; The polyacyl chloride is trimesoyl chloride, and the composition of the organic phase solution containing the polyacyl chloride includes: an Isopar G solution containing 0.05-0.5 wt % of trimesoyl chloride.

3. The preparation method according to claim 1, It is characterized in that The porous ultrafiltration membrane support layer is a polysulfone ultrafiltration membrane, and the pore size distribution of the porous ultrafiltration membrane support layer is 30 nm - 100 nm.

4. The preparation method according to claim 1, It is characterized in that The method of sequentially immersing the porous ultrafiltration membrane support layer in an aqueous solution containing a polyamine and an organic solution containing a polyacyl chloride so that the polyamine and the polyacyl chloride undergo an interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane specifically includes: After the porous ultrafiltration membrane support layer is contacted with the aqueous phase solution containing the polyamine according to a first contact condition, the porous ultrafiltration membrane support layer is contacted with the organic phase solution containing the polyacid chloride according to a second contact condition, and heat-treated according to a heat treatment condition, so that the polyamine and the polyacid chloride undergo an interfacial polymerization reaction to generate a polyamide separation layer of the nanofiltration membrane; in, The first contact condition is: contact time is 20-120s, contact temperature is 15-30°C; The second contact condition is: contact time is 20-120s, contact temperature is 15-30°C; The heat treatment conditions are: treatment temperature is 40-80°C, and treatment time is 2-10min.

5. The preparation method according to claim 1, It is characterized in that The solution for preparing the anti-organic pollution antibacterial ultra-thin layer comprises a polymer main material, a chelating agent and metal ions, wherein the polymer main material is a polyhydroxy polymer, the chelating agent is an amino polyacid, and the metal ions are copper ions or silver ions. The preparation process of the solution for preparing the anti-organic pollution antibacterial ultra-thin layer comprises: Dissolving the chelating agent in deionized water, adjusting the pH to 8.5, and adding the chelating agent to the soluble inorganic salt solution of the metal ion to generate a metal chelate solution; The metal chelate solution is added into the aqueous solution of the polymer main material, and the pH is adjusted to a preset pH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer.

6. The preparation method according to claim 5, It is characterized in that The polyhydroxy polymer is polyvinyl alcohol, and the concentration of the polyvinyl alcohol is 5-15 g / L; The amino polyacid is any one of ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, and triethylenetetraaminehexaacetic acid, and the concentration of the chelating agent is 5-15 mM; The concentration of the soluble inorganic salt in the soluble inorganic salt solution of metal ions is 5-15 mM.

7. The preparation method according to claim 5, It is characterized in that The preset pH is 8.0-9.0; The step of adding the metal chelate solution to the aqueous solution of the polymer main material and adjusting the pH to a preset pH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer specifically includes: The metal chelate solution is added into the aqueous solution of the polymer main material, and the pH is adjusted to 8.0-9.0 with NaOH to form the solution for preparing the anti-organic pollution antibacterial ultra-thin layer.

8. The preparation method according to claim 1, It is characterized in that The step of immersing the polyamide separation layer in a solution for preparing an ultra-thin layer against organic pollution and antibacterial properties to form an ultra-thin layer against organic pollution and antibacterial properties specifically comprises: The polyamide separation layer is immersed in the anti-organic pollution antibacterial thin layer preparation solution according to the third contact condition, and is dried to form the anti-organic pollution antibacterial ultra-thin layer.

9. The preparation method according to claim 8, It is characterized in that The third contact condition is: contact time is 1-10min, temperature is 25-35°C; The drying treatment adopts oven drying, and the oven drying conditions are: 60-100°C, 3-10 min.

10. A composite nanofiltration membrane with both anti-organic pollution and antibacterial properties, It is characterized in that The composite nanofiltration membrane is prepared by the preparation method according to any one of claims 1 to 9, and the composite nanofiltration membrane comprises: Porous ultrafiltration membrane support layer, polyamide separation layer and anti-organic pollution and antibacterial ultra-thin layer; in, The porous ultrafiltration membrane support layer is located at the bottom of the composite nanofiltration membrane, and the porous ultrafiltration membrane support layer is a polysulfone ultrafiltration membrane and / or a polyethersulfone ultrafiltration membrane; The polyamide separation layer is located in the middle of the composite nanofiltration membrane, and the polyamide separation layer covers the porous ultrafiltration membrane support layer; The anti-organic pollution and antibacterial ultra-thin layer is located on the top of the composite nanofiltration membrane, and is bonded to the polyamide separation layer through a covalent bond and attached to the polyamide separation layer. The anti-organic pollution and antibacterial ultra-thin layer is composed of a polymer main material, a chelating agent and antibacterial metal ions, and the polymer main material is connected to the chelating agent through a covalent bond, and the chelating agent is bonded to the antibacterial metal ions through a coordination bond.