Oil-water separation membrane as well as preparation method and application thereof

By introducing COFs materials and polyethyleneimine into the oil-water separation membrane, a film with underwater super oleophobic and antifouling properties is solved, and the problems of low permeability and susceptibility to contamination in the existing membrane are improved and separation efficiency is improved. The service life reduces operating costs.

CN118925522AActive Publication Date: 2024-11-12天津大学浙江研究院
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411080309.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

When the existing oil-water separation membranes treat oil-containing wastewater, the membrane permeability flux is low and susceptible to contamination, resulting in a decrease in separation efficiency and shortened service life, which increases operating costs.

Method used

Using the surface segregation method based on electrostatic reinforcement reaction, the separation membrane with underwater superoleophobic and antifouling properties is constructed by introducing covalent organic frames (COFs) materials as modifiers, combining polyethersulfone and polyethyleneimine, and optimized Mechanical strength and pore structure of the membrane.

Benefits of technology

It improves the anti-pollution performance and separation efficiency of the membrane, extends the service life of the membrane, and reduces operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925522A_ABST
    Figure CN118925522A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of water treatment, and provides an oil-water separation membrane as well as a preparation method and application thereof. The preparation method comprises the following steps: preparing negatively charged COFs powder; dissolving COFs powder, and mixing the dissolved COFs powder with polyether sulfone and polyethylene glycol to form a membrane casting solution; dissolving polyethyleneimine in water to prepare a coagulating bath; scraping the membrane casting solution on a glass plate to form a liquid membrane, and putting the liquid membrane into a coagulating bath for curing to form the membrane. The invention also discloses the oil-water separation membrane prepared by the method, and application of the oil-water separation membrane in oil-water separation. The polyether sulfone / COFs interface and the COFs pore channels in the separation membrane provide a large amount of confinement space, and the mass transfer mechanism in the membrane is optimized. The positively charged PEI enhances segregation of hydrophilic and negatively charged groups, and in-situ assembly is carried out in the phase inversion process to construct a selective separation layer. Ionic groups enriched on the surface of the membrane generate strong hydration, so that the membrane is endowed with underwater super-oleophobic and low-adhesion characteristics, and the anti-pollution mechanism of the surface of the membrane is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of water treatment, and in particular to an oil-water separation membrane and a preparation method and application thereof. Background Art

[0002] Oily wastewater is widely present in industrial production processes such as oil extraction and refining. It has a wide source, great harm, and complex composition. It is a type of wastewater that is difficult to treat. Developing efficient oil-water separation technology and realizing deep treatment and resource utilization of oily wastewater are of great significance to the development of green petrochemical industry. Compared with traditional oil-water separation technologies (flotation, flocculation, adsorption, etc.), membrane separation technology has low energy consumption and high separation efficiency, and has broad application prospects in the field of oily wastewater treatment. Research on high-performance oil-water separation membrane materials currently faces two common key problems: low membrane permeation flux and serious membrane pollution. Oil droplets are easy to adhere and spread on the membrane surface, causing serious and difficult-to-clean pollution on the membrane surface, resulting in a sharp drop in membrane flux, a decrease in separation efficiency, a shortened service life, and other problems, while increasing the overall operating cost.

[0003] Therefore, it is necessary to provide a separation membrane with underwater superoleophobic and antifouling properties. Summary of the invention

[0004] The present disclosure provides an oil-water separation membrane and a preparation method and application thereof, so as to at least solve the above technical problems existing in the prior art.

[0005] According to a first aspect of the present disclosure, a method for preparing an oil-water separation membrane is provided, comprising the following steps:

[0006] S1: mixing an amino monomer with an alkylpyridinium bromide solution to obtain a solution A; mixing trialdehyde phloroglucinol with dichloromethane to obtain a solution B; mixing the solution A and the solution B, precipitating, filtering, and obtaining a negatively charged COFs (covalent organic framework) powder;

[0007] S2: dissolving the COFs powder prepared in step S1 and mixing it with polyethersulfone and polyethylene glycol to form a casting solution; the mass ratio of the COFs powder to the polyethylene glycol is 0.1 to 3%;

[0008] S3: dissolving polyethyleneimine in water to prepare a coagulation bath; in the coagulation bath, the concentration of polyethyleneimine is 0 to 10 g / L;

[0009] S4: scraping the casting liquid prepared in step S2 onto a glass plate to form a liquid film, and then placing it into the solidification bath prepared in step S3 to solidify into a film, thereby obtaining the oil-water separation membrane.

[0010] In one embodiment, in the alkylpyridinium bromide solution of step S1, the alkylpyridinium bromide is selected from at least one of hexadecylpyridinium bromide and dodecylpyridinium bromide.

[0011] In a preferred embodiment, the alkylpyridinium bromide is selected from hexadecylpyridinium bromide.

[0012] In one embodiment, the alkylpyridinium bromide solution in step S1 is prepared by dissolving alkylpyridinium bromide in water, and the concentration of the alkylpyridinium bromide is 1 to 1.5 mg / mL.

[0013] In a preferred embodiment, the concentration of the alkylpyridinium bromide is 1 mg / mL.

[0014] In one embodiment, the amino monomer is selected from any one of Pa-PO3H2, Pa-SO3H, and Pa-CO2H.

[0015] In one embodiment, the concentration of the amino monomer is 1.5-2.0 mg / mL.

[0016] In a preferred embodiment, the concentration of the amino monomer is 1.6 mg / mL.

[0017] In one embodiment, in step S1, the amino monomer and the alkylpyridinium bromide solution are mixed at 500-800 rpm to obtain the solution A.

[0018] In a preferred embodiment, in step S1, the amino monomer and the alkylpyridinium bromide solution are mixed at 500 rpm to prepare the solution A.

[0019] In one embodiment, the concentration of the trialdehyde phloroglucinol is 8-10 mg / mL.

[0020] In a preferred embodiment, the concentration of trialdehyde phloroglucinol is 9 mg / mL.

[0021] In one embodiment, in step S1, the solution A and the solution B are mixed at room temperature for 10 to 15 minutes, solids are precipitated with ethanol, negatively charged COFs powder is filtered out, and purified with methanol.

[0022] In one embodiment, the specific step of dissolving the COFs powder in step S2 includes: adding the COFs powder into N,N-dimethylformamide solvent for dispersion.

[0023] In one embodiment, the mass ratio of the polyethersulfone to the N,N-dimethylformamide in step S2 is 1:(3.5-10).

[0024] In one embodiment, the polyethyleneimine has an average molecular weight of 70,000 to 75,000 and a solid content of 45 to 55%.

[0025] In a preferred embodiment, the polyethyleneimine has an average molecular weight of 70,000 and a solid content of 50%.

[0026] In one embodiment, in step S3, when the concentration of the polyethyleneimine is 0, the coagulation bath is water.

[0027] In a preferred embodiment, the concentration of polyethyleneimine in step S3 is 1-10 g / L.

[0028] In a more preferred embodiment, the concentration of polyethyleneimine in step S3 is 5 g / L.

[0029] In one possible implementation manner, the thickness of the liquid film in step S4 is 200-250 μm.

[0030] In a preferred embodiment, the thickness of the liquid film in step S4 is 200 μm.

[0031] In one possible implementation manner, in step S4, the casting liquid is scraped onto the glass plate to form the liquid film, and then placed in the solidification bath for 5 to 10 minutes to solidify into a film.

[0032] In one possible implementation manner, after the solidification into a film in step S4, the solid film is removed from the glass plate and then immersed in water for 12 to 24 hours to obtain the oil-water separation membrane.

[0033] According to a second aspect of the present disclosure, an oil-water separation membrane prepared according to the above preparation method is provided.

[0034] According to a third aspect of the present disclosure, there is provided an application of the above-mentioned oil-water separation membrane for oil-water separation in a light oil-water mixture, a heavy oil-water mixture, a water-in-oil emulsion, and an oil-in-water emulsion.

[0035] According to an implementable embodiment of the present disclosure, at least the following beneficial effects are achieved:

[0036] In view of the existing technology, constructing a super strong hydration layer on the membrane surface is an effective anti-pollution strategy. This disclosure proposes a separation membrane with underwater super oleophobic and anti-fouling properties based on an electrostatically enhanced reactive surface segregation method. By introducing COFs materials as modifiers, while achieving the modification of the membrane surface and pore structure, the mechanical strength of the membrane is improved and an additional pore structure is introduced.

[0037] The present invention uses emulsion polymerization to rapidly synthesize negatively charged COFs, and uses polymer as the main membrane material and COFs as a modifier. The polyethersulfone / COFs interface and COFs pores in the membrane provide a large amount of confined space, optimizing the mass transfer mechanism in the membrane.

[0038] In addition, due to the strong electrostatic force, the positively charged polyethyleneimine (PEI) in the coagulation bath enhances the segregation of hydrophilic and negatively charged groups in the casting solution, and in situ assembles and constructs a selective separation layer during the phase transformation process, which has the characteristics of simple operation, excellent membrane performance, and easy large-scale preparation. The ionic groups enriched on the membrane surface produce strong hydration, giving the membrane underwater superoleophobic and low adhesion properties, and strengthening the anti-fouling mechanism of the membrane surface.

[0039] It should be understood that the content described in this section is not intended to identify the key or important features of the embodiments of the present disclosure, nor is it intended to limit the scope of the present disclosure. Other features of the present disclosure will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The above and other objects, features and advantages of the exemplary embodiments of the present disclosure will become readily understood by reading the detailed description below with reference to the accompanying drawings. In the accompanying drawings, several embodiments of the present disclosure are shown in an exemplary and non-limiting manner, in which:

[0041] In the drawings, the same or corresponding reference numerals represent the same or corresponding parts.

[0042] Figure 1 shows the X-ray diffraction spectrum of TpPa-COOH powder in Example 1 of the present disclosure;

[0043] Figure 2 A cross-sectional scanning electron microscope image of the oil-water separation membrane 1 in Example 1 of the present disclosure is shown;

[0044] Figure 3 A cross-sectional scanning electron microscope image of a polyethersulfone membrane in a comparative example of the present disclosure is shown;

[0045] Figure 4 The permeation flux statistics of the separation membranes prepared in Examples 1 to 7 of the present disclosure and the comparative example are shown;

[0046] Figure 5 The statistical graph of flux recovery rate of the separation membranes prepared in Examples 1 to 7 of the present disclosure and the comparative example is shown. DETAILED DESCRIPTION

[0047] In order to make the purpose, features, and advantages of the present disclosure more obvious and easy to understand, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present disclosure.

[0048] At present, covalent organic framework materials (COFs) are developing rapidly. They have the characteristics of large specific surface area, high density of functional groups and high mechanical properties. They have the following potential advantages in the field of membrane separation: 1) COFs have high porosity, providing abundant transfer paths for material transfer within the membrane and obtaining high permeability; 2) COFs have uniform pore size, and the pore size can be precisely controlled by the structural design of the reaction monomer to achieve high selectivity; 3) COFs have a regular pore structure, and the wall contains high-density, uniformly distributed designable functional sites, and low-resistance walls can be designed to achieve rapid molecular transfer. These characteristics make COFs an ideal candidate material for preparing high-performance oil-water separation membranes, but there are currently only a few reports on COFs research in oil-water separation. Based on this, the present disclosure provides a separation membrane with underwater superoleophobic and antifouling properties prepared based on an electrostatically enhanced reactive surface segregation method. Specific analysis is combined with the following examples.

[0049] Example 1

[0050] In this embodiment, an oil-water separation membrane 1 is prepared, and the specific process is as follows:

[0051] (1) 15 mL of 1 mg / mL cetylpyridinium bromide aqueous solution was added to a round-bottom flask; 24 mg of amino monomer (2,5-diaminobenzoic acid) was added to the above cetylpyridinium bromide aqueous solution, and stirred at 500 rpm to dissolve, to prepare solution A; 31.5 mg of trialdehyde phloroglucinol was ultrasonically dissolved in 3.5 mL of dichloromethane to prepare solution B; solution A and solution B were mixed and stirred at room temperature for 10 min. After the reaction was completed, the solid was precipitated with ethanol, and the solid powder was filtered to obtain a negatively charged covalent organic framework (COFs) modifier, which was recorded as TpPa-COOH.

[0052] (2) 10 mg of the TpPa-COOH powder obtained in step (1) was added to 13.4 g of N,N-dimethylformamide solvent and dispersed evenly. Then, 3.6 g of polyethersulfone (BASF 6020, industrial grade) and 3 g of polyethylene glycol (molecular weight 600) were added and stirred to dissolve to form a casting solution.

[0053] (3) After cooling the casting liquid prepared in step (2) to room temperature, pour it onto a glass plate and scrape it into a liquid film about 200 μm thick, then put it into a coagulation bath of deionized water at 25°C for 5 minutes to solidify into a film, remove it from the glass plate and soak it in deionized water for 24 hours to obtain an oil-water separation membrane 1.

[0054] The XRD spectrum of the above TpPa-COOH powder is as follows: Figure 1 As shown, Figure 1 It was shown that the TpPa-COOH powder exhibited sharp diffraction peaks at 4.7°, 8.2°, 12.8°, and 27.1°, confirming the successful synthesis of TpPa-COOH.

[0055] The cross-sectional scanning electron microscope image of the oil-water separation membrane 1 is shown in FIG. Figure 2 As shown, Figure 2 The surface of the separation membrane is porous and the cross section shows a finger-like pore structure. The membrane pure water flux is 450Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween 80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 323Lm -2 h -1 bar -1 The interception rate is 99.5%. After washing with deionized water for 10 minutes, the anti-fouling index FRR is 89% (see Figure 5 , the flux recovery rate represents the anti-fouling index), which shows that the introduction of TpPa-COOH improves the anti-fouling performance of the membrane.

[0056] Comparative Example

[0057] This comparative example prepared a polyethersulfone membrane. The difference from Example 1 is that this comparative example did not introduce COFs to prepare the membrane casting solution. The specific process is:

[0058] 3.6g polyethersulfone (BASF 6020, industrial pure), 3g polyethylene glycol (molecular weight 600) and 13.4g N,N-dimethylformamide were added to a round-bottom flask, heated and stirred in a 60°C water bath for 6h, and then allowed to stand for degassing for 12h to obtain a casting solution. After the casting solution was cooled to room temperature, it was poured onto a glass plate and scraped into a liquid film of about 200μm thickness, placed in a coagulation bath of deionized water at 25°C, and cured for 5min to form a film. After being removed from the glass plate, it was soaked in deionized water for 24h to obtain a polyethersulfone membrane.

[0059] The cross-sectional scanning electron microscopy image of the polyethersulfone membrane is shown in FIG. Figure 3 As shown, Figure 3The surface is porous and the cross section is asymmetrical. The top surface has a dense cortex and the secondary layer has a finger-like pore structure that plays a supporting role. The pure water flux of the membrane is 366Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween 80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 293Lm -2 h -1 bar -1 The interception rate was 99.2%. After washing with deionized water for 10 minutes, the anti-pollution index FRR was 76% (see Figure 5 ), indicating that the anti-fouling performance of polyethersulfone membrane is weak.

[0060] Example 2

[0061] In this example, an oil-water separation membrane 2 was prepared. The specific process was basically the same as that of Example 1, except that the content of TpPa-COOH powder in step (2) was changed to 30 mg.

[0062] The results show that the surface of oil-water separation membrane 2 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 528Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 368Lm -2 h -1 bar -1 The interception rate is 99.5%. After washing with deionized water for 10 minutes, the anti-fouling index FRR is 91% (see Figure 5 ), indicating that the introduction of TpPa-COOH improves the anti-fouling performance of the membrane.

[0063] Example 3

[0064] In this example, an oil-water separation membrane 3 was prepared. The specific process was basically the same as that of Example 1, except that the content of TpPa-COOH powder in step (2) was changed to 50 mg.

[0065] The results show that the surface of oil-water separation membrane 3 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 412Lm -2 h -1 bar -1In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 210Lm -2 h -1 bar -1 The interception rate is 99.7%. After washing with deionized water for 10 minutes, the anti-pollution index FRR is 90% (see Figure 5 ), indicating that the introduction of TpPa-COOH improves the anti-fouling performance of the membrane.

[0066] Example 4

[0067] In this example, an oil-water separation membrane 4 was prepared. The specific process was basically the same as that of Example 1, except that the content of TpPa-COOH powder in step (2) was changed to 70 mg.

[0068] The results show that the surface of oil-water separation membrane 4 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 266Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 158Lm -2 h -1 bar -1 The interception rate is 99.6%. After washing with deionized water for 10 minutes, the anti-pollution index FRR is 90% (see Figure 5 ), indicating that the introduction of TpPa-COOH improves the anti-fouling performance of the membrane.

[0069] Example 5

[0070] In this embodiment, an oil-water separation membrane 5 is prepared, and the specific process is as follows:

[0071] (1) 15 mL of 1 mg / mL cetylpyridinium bromide aqueous solution was added to a round-bottom flask; 24 mg of amino monomer (2,5-diaminobenzoic acid) was added to the above cetylpyridinium bromide aqueous solution, and stirred at 500 rpm to dissolve, to prepare solution A; 31.5 mg of trialdehyde phloroglucinol was ultrasonically dissolved in 3.5 mL of dichloromethane to prepare solution B; solution A and solution B were mixed and stirred at room temperature for 10 min. After the reaction was completed, the solid was precipitated with ethanol, and the solid powder was filtered to obtain a negatively charged covalent organic framework (COFs) modifier, which was recorded as TpPa-COOH.

[0072] (2) 30 mg of the TpPa-COOH powder obtained in step (1) was added to 13.4 g of N,N-dimethylformamide solvent and dispersed evenly. Then, 3.6 g of polyethersulfone (BASF 6020, industrial grade) and 3 g of polyethylene glycol (molecular weight 600) were added and stirred to dissolve to form a casting solution.

[0073] (3) Add polyethyleneimine (PEI, average molecular weight 70,000, solid content 50%) into 1 L of deionized water and stir until fully dissolved to prepare a 1 g / L positively charged polyethyleneimine coagulation bath.

[0074] (4) After cooling the casting liquid prepared in step (2) to room temperature, pour it onto a glass plate and scrape it into a liquid film with a thickness of about 200 μm. Place it in the polyethyleneimine coagulation bath prepared in step (3) at a constant temperature of 25° C. and continue to solidify it for 5 minutes to form a film. After removing the solid film from the glass plate, soak it in deionized water for 24 hours to obtain an oil-water separation membrane 5.

[0075] The results show that the surface of oil-water separation membrane 5 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 552Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 393Lm -2 h -1 bar -1 The interception rate is 99.6%. After washing with deionized water for 10 minutes, the anti-pollution index FRR is 92% (see Figure 5 ), indicating that the introduction of TpPa-COOH and PEI improves the anti-fouling performance of the membrane.

[0076] Example 6

[0077] In this example, an oil-water separation membrane 6 was prepared. The specific process was basically the same as that of Example 5, except that the concentration of the positively charged polyethyleneimine coagulation bath in step (3) was changed to 5 g / L.

[0078] The results show that the surface of oil-water separation membrane 6 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 592Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 454Lm -2 h -1 bar-1 , the interception rate is 100%. After washing with deionized water for 10 minutes, the anti-fouling index FRR is 95% (see Figure 5 ), indicating that the introduction of TpPa-COOH and PEI improves the anti-fouling performance of the membrane.

[0079] Example 7

[0080] In this embodiment, an oil-water separation membrane 7 is prepared. The specific process is basically the same as that of Example 5, except that the concentration of the positively charged polyethyleneimine coagulation bath in step (3) is changed to 10 g / L.

[0081] The results show that the surface of oil-water separation membrane 7 is porous and the cross section shows a finger-like pore structure. The pure water flux of the membrane is 446Lm -2 h -1 bar -1 In the oil-water emulsion (0.1wt% pump oil, 0.01wt% Tween80, 99.89wt% water) separation application, the membrane permeation flux data can be found in Figure 4 , its value is 348Lm -2 h -1 bar -1 , the interception rate is 100%. After washing with deionized water for 10 minutes, the anti-fouling index FRR is 95% (see Figure 5 ), indicating that the introduction of TpPa-COOH and PEI improves the anti-fouling performance of the membrane.

[0082] In summary, the preparation method provided by the present disclosure can form a membrane through a one-step method, and the anti-fouling structural layer on the membrane surface can be regulated by adjusting the amount of TpPa-COOH added in the casting solution and the concentration of polyethyleneimine in the coagulation bath. The addition of polyethyleneimine in the coagulation bath enhances the anti-fouling performance of the membrane surface. As the concentration of polyethyleneimine increases, the permeation flux of the oil-water separation membrane first increases and then decreases, the interception rate remains basically unchanged, and the anti-fouling performance is improved. The comprehensive performance of the oil-water separation membrane 6 prepared in Example 6 reaches the optimal value.

[0083] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps recorded in this disclosure can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of this disclosure can be achieved, and this document is not limited here.

[0084] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0085] The above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A method for preparing an oil-water separation membrane, characterized in that: The following steps are involved: S1: mixing an amino monomer with an alkylpyridinium bromide solution to obtain a solution A; mixing trialdehyde phloroglucinol with dichloromethane to obtain a solution B; mixing the solution A and the solution B, precipitating, filtering, and obtaining a negatively charged COFs powder; S2: dissolving the COFs powder prepared in step S1 and mixing it with polyethersulfone and polyethylene glycol to form a casting solution; the mass ratio of the COFs powder to the polyethylene glycol is 0.1 to 3%; S3: dissolving polyethyleneimine in water to prepare a coagulation bath; in the coagulation bath, the concentration of polyethyleneimine is 0 to 10 g / L; S4: scraping the casting liquid prepared in step S2 onto a glass plate to form a liquid film, and then placing it into the solidification bath prepared in step S3 to solidify into a film, thereby obtaining the oil-water separation membrane.

2. The preparation method according to claim 1, characterized in that: In the alkylpyridinium bromide solution of step S1, the alkylpyridinium bromide is selected from at least one of hexadecylpyridinium bromide and dodecylpyridinium bromide; Preferably, the amino monomer is selected from any one of Pa-PO3H2, Pa-SO3H, and Pa-CO2H; Preferably, in step S1, the amino monomer and the alkylpyridinium bromide solution are mixed at 500-800 rpm to obtain the solution A; Preferably, in step S1, the solution A and the solution B are mixed at room temperature for 10 to 15 minutes, solids are precipitated with ethanol, negatively charged COFs powder is filtered out, and purified with methanol.

3. The preparation method according to claim 1, characterized in that: The specific steps of step S2 dissolving the COFs powder include: adding the COFs powder into N,N-dimethylformamide solvent for dispersion; Preferably, in step S2, the mass ratio of the polyethersulfone to the N,N-dimethylformamide is 1:(3.5-10).

4. The preparation method according to claim 1, characterized in that: The average molecular weight of the polyethyleneimine is 70,000-75,000, and the solid content is 45-55%.

5. The preparation method according to claim 1, characterized in that: In step S3, when the concentration of the polyethyleneimine is 0, the coagulation bath is water.

6. The preparation method according to claim 1, characterized in that: The concentration of the polyethyleneimine in step S3 is 1-10 g / L.

7. The preparation method according to claim 1, characterized in that: The thickness of the liquid film in step S4 is 200-250 μm.

8. The preparation method according to claim 1, characterized in that: Step S4: scraping the casting liquid onto the glass plate to form the liquid film, and then placing the liquid film into the solidification bath for 5 to 10 minutes to solidify into a film; Preferably, in step S4, after the solidification into a film, the solid film is removed from the glass plate and then immersed in water for 12 to 24 hours to obtain the oil-water separation membrane.

9. The oil-water separation membrane obtained according to the preparation method according to any one of claims 1 to 8.

10. Use of the oil-water separation membrane of claim 9 for oil-water separation in light oil-water mixtures, heavy oil-water mixtures, water-in-oil emulsions, and oil-in-water emulsions.

Citation Information

Patent Citations

  • Thin film nanocomposite membranes containing metal-organic cages for desalination

    CN112055609A

  • One-dimensional nano-channel self-supporting covalent organic framework membrane for salinity gradient power generation, and application thereof

    CN113461887A

  • Polyelectrolyte / covalent organic framework nanosheet hybrid membrane as well as preparation method and application thereof

    CN116236918A

  • Preparation method of COFs / PAN oil-water separation microporous membrane with submerged super-amphiphobic property

    CN116764459A

  • PSPEEK / COF composite membrane for reverse electrodialysis technology and preparation method of PSPEEK / COF composite membrane

    CN117085517A