Anti-biodegradation water-stable cellulose acetate fiber filtering membrane and preparation method thereof
By forming quaternary ammonium and Schiff alkali structures in cellulose acetate filter membranes, and deposition of nanosilver particles using ultraviolet light and atomized silver ions, the shortcomings of existing antibacterial filter membranes in biodegradation and water stability are solved, and the problem of achieving the goal of achieving It has efficient antibacterial and improved stability, and is suitable for filtration of complex water environments.
Patent Information
- Application Number
- CN202410927695.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing antibacterial filter membranes are insufficient in the face of biodegradation, making it difficult to maintain long-term antibacterial performance, and the water stability is poor, which cannot effectively solve the filtration problem of pollutants.
The reaction of 4-dimethylaminomethyl-benzaldehyde and 3-chloro-N-propyl-2-enyl-propylamide to form a quaternary ammonium structure, and the combination of aldehyde groups and 3-aminopropylene forms a Schiff base, and grafts it on Cellulose acetate is electrospinned and ultraviolet light is irradiated to form a rich three-dimensional network structure, and nano-silver particles are deposited using atomized silver ions to enhance the antibacterial and stability of the film.
It significantly improves the anti-biodegradability and water stability of the filter membrane, enhances the killing ability of bacteria of different sizes, maintains the overall structural stability of the membrane, and improves the filtration performance.
Smart Images

Figure BDA0004938716150000061 
Figure BDA0004938716150000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of membrane technology, in particular to an anti-biodegradation water-stable cellulose acetate filter membrane and a preparation method thereof. Background Art
[0002] Membrane separation technology has the functions of separation, purification, concentration and refinement, and has the characteristics of high efficiency, energy saving, environmental protection, high separation accuracy and easy integration. It is widely used in water treatment, chemical industry, environmental protection, food, medicine and other fields.
[0003] In order to improve the fouling resistance of membrane materials, by giving the filter membrane antibacterial properties, antibacterial agents are usually introduced on the surface of the filter membrane to inhibit the growth of bacteria on the membrane surface or even kill the bacteria, thus giving it antibacterial properties. Summary of the invention
[0004] The object of the present invention is to provide a biodegradable water-stable cellulose acetate filter membrane and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a biodegradable water-stable cellulose acetate filter membrane, comprising the following preparation steps:
[0006] (1) 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide were mixed, reacted at 40-60°C for 72 hours, cooled to room temperature, added with ethyl acetate, filtered, and dissolved in anhydrous methanol 3-5 times the mass of 4-dimethylaminomethyl-benzaldehyde, and then ethyl acetate was added for precipitation. The mixture was stirred at 80 rpm for 30 minutes, filtered, and dried to obtain a quaternary ammonium compound;
[0007] (2) 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol are mixed, reacted at 40-55° C. for 2 h, dried at 55° C. and vacuum degree of -0.08 MPa until no solution is present, washed with ice ethanol three times, filtered, and the filter cake is dried to obtain an antibacterial modifier;
[0008] (3) Mix cellulose acetate and deionized water in a ratio of 10 g:120 mL, add cerium ammonium nitrate in a ratio of 0.08 to 0.1 times the mass of cellulose acetate under a nitrogen atmosphere, stir evenly, add 1 mol / L nitric acid aqueous solution in a ratio of 10 g:20 mL, react at 60° C. and 60 rpm for 30 to 50 min, add an antibacterial modifier in a ratio of 0.2 to 0.3 times the mass of cellulose acetate, continue stirring and reacting for 12 h, let stand for 1 h, remove the upper layer of liquid, wash the lower layer of powdered product with anhydrous ethanol for 3 to 6 times, and dry at 60° C. for 24 h to obtain modified cellulose acetate;
[0009] (4) dissolving modified cellulose acetate, ammonium persulfate, and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylacetamide and acetone, wherein the volume ratio of N,N-dimethylacetamide to acetone is 3:2, and heating at 60° C. and 80 rpm for 6 h to obtain a spinning solution;
[0010] (5) The spinning solution was loaded into a 6 mL syringe with a needle inner diameter of 0.41 mm. The syringe was fixed on a syringe pump with a propulsion speed of 1 mL / h. The electrospinning voltage was set to 18 kV, the distance between the needle tip and the receiver was 20 cm, the relative humidity during the spinning process was 25-30%, and a UV lamp with a wavelength of 172 nm was used to irradiate at 40°C for 6 h to obtain a fiber membrane;
[0011] (6) The fiber membrane is placed in an atomizing device, and a 0.05 mol / L silver nitrate aqueous solution is used as the atomizing liquid. The atomizing flow rate is 200-300 mL / h, and the atomizing time is 30-40 min. The introduction of the atomizing liquid is stopped, and an ultraviolet lamp with a wavelength of 172 nm is used to irradiate the membrane at 40° C. for 24 h to obtain a biodegradable water-stable cellulose acetate filter membrane.
[0012] Furthermore, in step (1), the ratio of 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide is 1-1.2 g:20 mL:3-5 g.
[0013] Furthermore, the volume ratio of ethyl acetate to methanol in step (1) is 20:1.
[0014] Furthermore, the drying conditions in step (1) are: temperature of 70° C. and time of 24 h.
[0015] Furthermore, in step (2), the ratio of 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol is 150-170 mg: 50-60 mg: 15 mL.
[0016] Furthermore, the drying conditions in step (2) are: temperature of 70° C. and time of 6 h.
[0017] Furthermore, in step (4), the mass fraction of the modified cellulose acetate in the spinning solution is 6 to 10 wt%.
[0018] Furthermore, the mass fraction of the polyvinyl pyrrolidone in the spinning solution in step (4) is 10 to 30 wt%.
[0019] Furthermore, in step (4), the mass fraction of the ammonium persulfate in the spinning solution is 0.01 to 0.2 wt%.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] The invention utilizes the dimethylamino group of 4-dimethylaminomethyl-benzaldehyde to react with the chlorine group of 3-chloro-N-prop-2-enyl-propionamide to form a quaternary ammonium structure to achieve the antibacterial property of the fiber filter membrane, then utilizes the aldehyde group of 4-dimethylaminomethyl-benzaldehyde to react with 3-aminopropylene to form a Schiff base structure, which acts together with the quaternary ammonium structure to improve the antibacterial property of the antibacterial membrane, thereby effectively killing bacteria of different sizes remaining in the liquid and playing a filtering role, then utilizes double bonds to be grafted into the side chains of cellulose acetate molecules to give the cellulose acetate antibacterial property, then electrostatically spins the filter membrane, and when it is not completely dried, performs ultraviolet irradiation to promote further polymerization of double bond free radicals, enrich the internal network structure of the fiber, and even if some components are degraded, the three-dimensional network structure of the filter membrane still maintains integrity, thereby improving the stability of the filter membrane, and improving the anti-biodegradability and water stability of the filter membrane.
[0022] Silver ions are deposited on the surface of the filter membrane by atomization. The nano droplets formed by atomization can effectively infiltrate the surface of the filter membrane and are conducive to the subsequent formation of nano silver particles with good dispersion. Then, a second ultraviolet light irradiation is carried out to generate nano Ag particles on the surface of the filter membrane, which provide support for the filter membrane and thus improve the stability and antibacterial properties of the filter membrane. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe the method in detail. The test methods for the various indicators of the filter membranes prepared in the following examples are as follows:
[0025] Anti-biodegradability: Prepare 10000 units / mL of lysozyme phosphate buffer and dispense it into 7 small triangular flasks, each containing 100 mL of lysozyme solution. Place the filter membranes of the embodiment and comparative example into the triangular flasks containing the lysozyme solution, respectively, and carry out degradation determination in a constant temperature box at 37°C. Take out and weigh the membranes every 10 days to calculate the degradation rate.
[0026] Filtration: The water flux was tested at 0.1MPa. Nano-colorant red pigment particles with a particle size distribution of 50-300nm were used as the filtration medium to test the filtration efficiency of the first 10s and 60s of the filtration experiment. The pure water flux was 2000L / m 2 h.
[0027] Antibacterial: The antibacterial properties are determined according to GB / T20944.2-2007.
[0028] Example 1
[0029] (1) 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide were mixed in a ratio of 1g:20mL:3g, reacted at 40°C for 72h, cooled to room temperature, added with ethyl acetate 20 times the volume of methanol, filtered out, and dissolved in anhydrous methanol 3 to 5 times the mass of 4-dimethylaminomethyl-benzaldehyde, and then added with ethyl acetate for precipitation, stirred at 80rpm for 30min, filtered out the filter cake, and dried at 70°C for 24h to obtain a quaternary ammonium compound;
[0030] (2) 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol were mixed in a ratio of 150 mg:50 mg:15 mL, reacted at 40° C. for 2 h, dried at 55° C. and vacuum degree -0.08 MPa until no solution was present, washed with ice ethanol three times, filtered, and the filter cake was dried at 70° C. for 6 h to obtain an antibacterial modifier;
[0031] (3) Cellulose acetate and deionized water were mixed in a ratio of 10 g:120 mL, and 0.08 times the mass of cerium ammonium nitrate of cellulose acetate was added under nitrogen atmosphere. After stirring evenly, 1 mol / L nitric acid aqueous solution was added in a ratio of 10 g:20 mL, and the mixture was reacted at 60° C. and 60 rpm for 30 min. An antibacterial modifier of 0.2 times the mass of cellulose acetate was added, and the mixture was stirred and reacted for 12 h. The mixture was allowed to stand for 1 h, and the upper layer of liquid was removed. The powdery product in the lower layer was washed with anhydrous ethanol for 3 times, and dried at 60° C. for 24 h to obtain modified cellulose acetate.
[0032] (4) dissolving modified cellulose acetate, ammonium persulfate and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylacetamide and acetone, wherein the volume ratio of N,N-dimethylacetamide to acetone is 3:2, and heating at 60° C. and 80 rpm for 6 hours with stirring to obtain a spinning solution; wherein the mass fraction of the modified cellulose acetate in the spinning solution is 6wt%, the mass fraction of the polyvinyl pyrrolidone in the spinning solution is 10wt%, and the mass fraction of the ammonium persulfate in the spinning solution is 0.01wt%;
[0033] (5) The spinning solution was loaded into a 6 mL syringe with a needle inner diameter of 0.41 mm. The syringe was fixed on a syringe pump with a propulsion speed of 1 mL / h. The electrospinning voltage was set to 18 kV, the distance between the needle tip and the receiver was 20 cm, the relative humidity during the spinning process was 25%, and a UV lamp with a wavelength of 172 nm was used to irradiate at 40°C for 6 h to obtain a fiber membrane;
[0034] (6) The fiber membrane was placed in an atomizing device, and a 0.05 mol / L silver nitrate aqueous solution was used as the atomizing liquid. The atomizing flow rate was 200 mL / h, and the atomizing time was 30 min. The introduction of the atomizing liquid was stopped, and an ultraviolet lamp with a wavelength of 172 nm was used to irradiate the membrane at 40° C. for 24 h to obtain a biodegradable water-stable cellulose acetate filter membrane.
[0035] Example 2
[0036] (1) 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide were mixed in a ratio of 1.1 g:20 mL:4 g, reacted at 50° C. for 72 h, cooled to room temperature, added with ethyl acetate in an amount 20 times the volume of methanol, filtered out, and dissolved in anhydrous methanol in an amount 4 times the mass of 4-dimethylaminomethyl-benzaldehyde. Ethyl acetate was then added for precipitation, stirred at 80 rpm for 30 min, filtered out the filter cake, and dried at 70° C. for 24 h to obtain a quaternary ammonium compound;
[0037] (2) 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol were mixed in a ratio of 160 mg:55 mg:15 mL, reacted at 48° C. for 2 h, dried at 55° C. and vacuum degree of -0.08 MPa until no solution was present, washed with ice ethanol three times, filtered, and the filter cake was dried at 70° C. for 6 h to obtain an antibacterial modifier;
[0038] (3) Cellulose acetate and deionized water were mixed in a ratio of 10 g:120 mL, and 0.09 times the mass of cerium ammonium nitrate of cellulose acetate was added under nitrogen atmosphere. After stirring evenly, 1 mol / L nitric acid aqueous solution was added in a ratio of 10 g:20 mL, and the mixture was reacted at 60° C. and 60 rpm for 40 min. An antibacterial modifier of 0.25 times the mass of cellulose acetate was added, and the mixture was stirred and reacted for 12 h. The mixture was allowed to stand for 1 h, and the upper layer of liquid was removed. The powdered product in the lower layer was washed with anhydrous ethanol for 5 times, and dried at 60° C. for 24 h to obtain modified cellulose acetate.
[0039] (4) dissolving modified cellulose acetate, ammonium persulfate and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylacetamide and acetone, wherein the volume ratio of N,N-dimethylacetamide to acetone is 3:2, and heating at 60° C. and 80 rpm for 6 hours with stirring to obtain a spinning solution; wherein the mass fraction of the modified cellulose acetate in the spinning solution is 8wt%, the mass fraction of the polyvinyl pyrrolidone in the spinning solution is 20wt%, and the mass fraction of the ammonium persulfate in the spinning solution is 0.12wt%;
[0040] (5) The spinning solution was loaded into a 6 mL syringe with a needle inner diameter of 0.41 mm. The syringe was fixed on a syringe pump with a propulsion speed of 1 mL / h. The electrospinning voltage was set to 18 kV, the distance between the needle tip and the receiver was 20 cm, the relative humidity during the spinning process was 28%, and a UV lamp with a wavelength of 172 nm was used to irradiate at 40°C for 6 h to obtain a fiber membrane;
[0041] (6) The fiber membrane was placed in an atomizing device, and a 0.05 mol / L silver nitrate aqueous solution was used as the atomizing liquid. The atomizing flow rate was 250 mL / h, and the atomizing time was 35 min. The introduction of the atomizing liquid was stopped, and an ultraviolet lamp with a wavelength of 172 nm was used to irradiate the membrane at 40° C. for 24 h to obtain a biodegradable water-stable cellulose acetate filter membrane.
[0042] Example 3
[0043] (1) 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide were mixed in a ratio of 1.2 g:20 mL:5 g, reacted at 60° C. for 72 h, cooled to room temperature, added with ethyl acetate in an amount 20 times the volume of methanol, filtered out, and dissolved in anhydrous methanol in an amount 5 times the mass of 4-dimethylaminomethyl-benzaldehyde, and then added with ethyl acetate for precipitation, stirred at 80 rpm for 30 min, filtered out the filter cake, and dried at 70° C. for 24 h to obtain a quaternary ammonium compound;
[0044] (2) 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol were mixed in a ratio of 170 mg:60 mg:15 mL, reacted at 55° C. for 2 h, dried at 55° C. and vacuum degree -0.08 MPa until no solution was present, washed with ice ethanol three times, filtered, and the filter cake was dried at 70° C. for 6 h to obtain an antibacterial modifier;
[0045] (3) Cellulose acetate and deionized water were mixed in a ratio of 10 g:120 mL, and 0.1 times the mass of cerium ammonium nitrate of cellulose acetate was added under nitrogen atmosphere. After stirring evenly, 1 mol / L nitric acid aqueous solution was added in a ratio of 10 g:20 mL, and the mixture was reacted at 60° C. and 60 rpm for 50 min. An antibacterial modifier of 0.3 times the mass of cellulose acetate was added, and the mixture was stirred and reacted for 12 h. The mixture was allowed to stand for 1 h, and the upper layer of liquid was removed. The powdered product in the lower layer was washed with anhydrous ethanol for 6 times, and dried at 60° C. for 24 h to obtain modified cellulose acetate.
[0046] (4) dissolving modified cellulose acetate, ammonium persulfate and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylacetamide and acetone, wherein the volume ratio of N,N-dimethylacetamide to acetone is 3:2, and heating at 60° C. and 80 rpm for 6 hours to obtain a spinning solution; the mass fraction of the modified cellulose acetate in the spinning solution is 10 wt %, the mass fraction of the polyvinyl pyrrolidone in the spinning solution is 30 wt %, and the mass fraction of the ammonium persulfate in the spinning solution is 0.2 wt %;
[0047] (5) The spinning solution was loaded into a 6 mL syringe with a needle inner diameter of 0.41 mm. The syringe was fixed on a syringe pump with a propulsion speed of 1 mL / h. The electrospinning voltage was set to 18 kV, the distance between the needle tip and the receiver was 20 cm, the relative humidity during the spinning process was 30%, and a UV lamp with a wavelength of 172 nm was used to irradiate at 40°C for 6 h to obtain a fiber membrane;
[0048] (6) The fiber membrane was placed in an atomizing device, and a 0.05 mol / L silver nitrate aqueous solution was used as the atomizing liquid. The atomizing flow rate was 300 mL / h, and the atomizing time was 40 min. The introduction of the atomizing liquid was stopped, and an ultraviolet lamp with a wavelength of 172 nm was used to irradiate the membrane at 40° C. for 24 h to obtain a biodegradable water-stable cellulose acetate filter membrane.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 2 is that 3-chloro-N-prop-2-enyl-propionamide is not added, and the remaining steps are the same as Example 2.
[0051] Comparative Example 2
[0052] The difference between Comparative Example 2 and Example 2 is that 3-aminopropylene is not added, and the remaining steps are the same as Example 2.
[0053] Comparative Example 3
[0054] The difference between Comparative Example 3 and Example 2 is that the first ultraviolet irradiation is not performed, and the remaining steps are the same as Example 2.
[0055] Comparative Example 4
[0056] The difference between Comparative Example 4 and Example 2 is that the second ultraviolet light irradiation is not performed, and the remaining steps are the same as Example 2.
[0057] Effect example
[0058] Table 1 below shows the performance analysis results of the filtration membranes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.
[0059] Table 1
[0060]
[0061]
[0062] The present invention utilizes the dimethylamino group of 4-dimethylaminomethyl-benzaldehyde to react with the chlorine group of 3-chloro-N-prop-2-enyl-propionamide to form a quaternary ammonium structure to achieve the antibacterial property of the fiber filter membrane, and then utilizes the aldehyde group of 4-dimethylaminomethyl-benzaldehyde to react with 3-aminopropylene to form a Schiff base structure, which acts together with the quaternary ammonium structure to improve the antibacterial performance of the antibacterial membrane, thereby effectively killing bacteria of different sizes remaining in the liquid and playing a filtering role, and then utilizes double bonds to graft into the side chains of cellulose acetate molecules to give the cellulose acetate antibacterial property, and then electrospins into a filter membrane, and when it is not completely dried, Ultraviolet light is applied to promote further polymerization of double-bond free radicals and enrich the internal network structure of the fiber. Even if some components are degraded, the three-dimensional network structure of the filter membrane still maintains its integrity, thereby improving the stability of the filter membrane and improving the filter membrane's anti-biodegradability and water stability. Atomization is then used to deposit silver ions on the filter membrane surface. The nano droplets formed by atomization can effectively infiltrate the filter membrane surface and are conducive to the subsequent formation of nano silver particles with good dispersion. Then, a second ultraviolet light irradiation is performed, and nano Ag particles are generated on the filter membrane surface to provide support for the filter membrane, thereby improving the stability and antibacterial properties of the filter membrane.
[0063] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a biodegradable water-stable cellulose acetate filter membrane, characterized in that: The method comprises the following preparation steps: (1) 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide were mixed, reacted at 40-60°C for 72 hours, cooled to room temperature, added with ethyl acetate, filtered, and dissolved in anhydrous methanol 3-5 times the mass of 4-dimethylaminomethyl-benzaldehyde, and then ethyl acetate was added for precipitation. The mixture was stirred at 80 rpm for 30 minutes, filtered, and dried to obtain a quaternary ammonium compound; (2) 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol are mixed, reacted at 40-55° C. for 2 h, dried at 55° C. and vacuum degree of -0.08 MPa until no solution is present, washed with ice ethanol three times, filtered, and the filter cake is dried to obtain an antibacterial modifier; (3) Mix cellulose acetate and deionized water in a ratio of 10 g:120 mL, add cerium ammonium nitrate in a ratio of 0.08 to 0.1 times the mass of cellulose acetate under a nitrogen atmosphere, stir evenly, add 1 mol / L nitric acid aqueous solution in a ratio of 10 g:20 mL, react at 60° C. and 60 rpm for 30 to 50 min, add an antibacterial modifier in a ratio of 0.2 to 0.3 times the mass of cellulose acetate, continue stirring and reacting for 12 h, let stand for 1 h, remove the upper layer of liquid, wash the lower layer of powdered product with anhydrous ethanol for 3 to 6 times, and dry at 60° C. for 24 h to obtain modified cellulose acetate; (4) dissolving modified cellulose acetate, ammonium persulfate, and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylacetamide and acetone, wherein the volume ratio of N,N-dimethylacetamide to acetone is 3:2, and heating at 60° C. and 80 rpm for 6 h to obtain a spinning solution; (5) The spinning solution was loaded into a 6 mL syringe with a needle inner diameter of 0.41 mm. The syringe was fixed on a syringe pump with a propulsion speed of 1 mL / h. The electrospinning voltage was set to 18 kV, the distance between the needle tip and the receiver was 20 cm, the relative humidity during the spinning process was 25-30%, and a UV lamp with a wavelength of 172 nm was used to irradiate at 40°C for 6 h to obtain a fiber membrane; (6) The fiber membrane is placed in an atomizing device, and a 0.05 mol / L silver nitrate aqueous solution is used as the atomizing liquid. The atomizing flow rate is 200-300 mL / h, and the atomizing time is 30-40 min. The introduction of the atomizing liquid is stopped, and an ultraviolet lamp with a wavelength of 172 nm is used to irradiate the membrane at 40° C. for 24 h to obtain a biodegradable water-stable cellulose acetate filter membrane.
2. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The ratio of 4-dimethylaminomethyl-benzaldehyde, methanol and 3-chloro-N-prop-2-enyl-propionamide in step (1) is 1-1.2 g:20 mL:3-5 g.
3. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The volume ratio of ethyl acetate to methanol in step (1) is 20:
1.
4. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The drying conditions in step (1) are: temperature of 70° C. and time of 24 h.
5. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The ratio of 4-dimethylaminomethyl-benzaldehyde, quaternary ammonium compound and anhydrous ethanol in step (2) is 150-170 mg: 50-60 mg: 15 mL.
6. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The drying conditions in step (2) are: temperature of 70° C. and time of 6 h.
7. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The mass fraction of the modified cellulose acetate in the spinning solution in step (4) is 6 to 10 wt%.
8. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The mass fraction of the polyvinyl pyrrolidone in the spinning solution in step (4) is 10 to 30 wt%.
9. The method for preparing a biodegradable water-stable cellulose acetate filter membrane according to claim 1, characterized in that: The mass fraction of the ammonium persulfate in the spinning solution in step (4) is 0.01 to 0.2 wt%.
Citation Information
Patent Citations
Preparation method for modified polyvinylpyrrolidone / cellulose acetate nanofiber membrane
CN102409484A
Preparation method of high-adsorbability cellulose diacetate composite electrostatic spinning nanofiber ordered porous film
CN105396563A
Antimicrobial modification method of cellulose acetate nano fiber
CN106637461A
Antibacterial material for pediatric pneumonia protection and manufacturing method thereof
CN111235661A
Method of producing high-washability acetatetextiles for retaining antibacterial function
KR1020040042568A