Ceramic micro-nanofiber aerogel material as well as preparation method and application thereof
By introducing a second silicon source and controlling the stirring conditions, the problem of short spinning window period of precursor solution was solved, and the production efficiency and thermal insulation performance of ceramic micro/nanofiber aerogel materials were improved.
Patent Information
- Application Number
- CN202410999394.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
In existing preparation methods, the spinning window of the PVP/TEOS precursor solution is short, leading to frequent solution changes and limiting the production efficiency of ceramic micro/nanofiber aerogel materials.
A precursor solution preparation method comprising a first silicon source and a second silicon source is adopted. By introducing a second silicon source such as 3-aminopropyltrimethoxysilane or γ-glycidoxypropyltrimethoxysilane, combined with specified stirring speed and temperature control, the stability and uniformity of the solution are ensured, and the spinning window period is extended.
It effectively extends the spinning window period of the precursor solution, improves production efficiency, and produces ceramic micro/nanofiber aerogel materials with low fiber density and finer fiber diameter, exhibiting good thermal insulation properties.
Smart Images

Figure CN118925609A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of micro-nano fiber materials, and in particular to a ceramic micro-nano fiber aerogel material and a preparation method and application thereof. Background Art
[0002] Micro-nano fiber aerogel is a new type of high-performance fiber. It is an ultra-light and porous new type of high-performance fiber directly obtained through sol-gel spinning and special drying technology. Micro-nano fiber aerogel combines aerogel and nanofiber technology, and has the advantages of both. It is the perfect embodiment of aerogel structure in fiber materials. Micro-nano fiber aerogel has the characteristics of high porosity, low density, excellent thermal insulation and adsorption capacity, and is widely used in energy storage, sound insulation, catalysis, filtration and other fields.
[0003] Centrifugal spinning technology is a common method for preparing nano-scale fiber materials. During the centrifugal spinning process, a polymer solution is injected into the liquid storage mechanism of the spinning disk and sprayed out through a needle. Then, under the action of the rotating centrifugal force, the polymer solution will be stretched into extremely fine fibers, which are finally deposited and collected on a collecting net to form a nano-scale fiber membrane or fiber bundle.
[0004] TEOS, or tetraethyl silicate, is a commonly used silicon source and is widely used in the preparation of SiO2 fiber aerogel. SiO2 fiber aerogel uses PVP / TEOS system as a precursor, and centrifugal spinning technology can be used to prepare SiO2 fiber aerogel with low thermal conductivity. However, in the existing preparation method, the PVP / TEOS precursor solution has a limited time to maintain spinnability during the spinning process, and usually loses spinnability within 1 hour after the precursor solution is completely hydrolyzed. The spinning window period of the PVP / TEOS precursor solution is short and the stability is poor. In the process of preparing ceramic micro-nano fiber aerogel materials, if the precursor solution loses its spinnability, it is necessary to remove the precursor solution in the liquid storage tank, and reconfigure and fill it with a new precursor solution, which greatly limits the production efficiency. Summary of the invention
[0005] The purpose of the present invention is to provide a ceramic micro-nano fiber aerogel material and a preparation method and application thereof, so as to solve the problem that the spinning window period of the precursor solution in the existing preparation method is short and the precursor solution needs to be frequently replaced.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for preparing a ceramic micro-nano fiber aerogel material. The ceramic micro-nano fiber aerogel material is prepared from a precursor solution, wherein the precursor solution comprises a polymer, a first silicon source, a second silicon source and a catalyst; the second silicon source comprises one of a silane having three oxygen groups and a silane having two oxygen groups; the preparation method comprises the following steps:
[0008] Prepare a polymer solution: dissolve the polymer in a solvent, and stir at a first stirring speed for a first stirring time until the solution is uniform to form a polymer solution;
[0009] Preparing a precursor solution: adding a first silicon source and a second silicon source to a polymer solution, stirring at a second stirring speed, adding a catalyst dropwise during the stirring process, and standing after a second stirring time to obtain a precursor solution;
[0010] Preparing a precursor: spinning a spinnable precursor solution into solid micro-nano fibers using a spinning device, and the micro-nano fibers are accumulated on a collecting device to form fibers, thereby obtaining a ceramic micro-nano fiber aerogel precursor;
[0011] Sintering precursor: putting the ceramic micro-nano fiber aerogel precursor into a boiler for sintering, the sintering temperature is 950-1100° C., the sintering time is 0.8-1.2 hours, and the ceramic micro-nano fiber aerogel material is obtained by sintering.
[0012] In the preparation method of the ceramic micro-nano fiber aerogel material, the first silicon source is tetraethyl silicate, and the second silicon source includes one of 3-aminopropyltrimethoxysilane (APMTS), γ-glycidyloxypropyltrimethoxysilane (GPTMS), dimethyldimethoxysilane (DMDMS) and methyltrimethoxysilane (MTMS).
[0013] In the preparation method of the ceramic micro-nano fiber aerogel material, the concentration of the polymer is 0.0007-0.0013 mol / L; the concentration of the first silicon source is 0.96-1.20 mol / L; the concentration of the second silicon source is 0.18-0.48 mol / L; and the concentration of the catalyst is 0.15-0.25 mol / L.
[0014] In the method for preparing the ceramic micro-nano fiber aerogel material, the molar ratio of the first silicon source to the second silicon source is 7:1 to 1:1.
[0015] In the method for preparing the ceramic micro-nano fiber aerogel material, in the step of preparing the precursor solution, the polymer solution is placed in an environment of 25-40° C. and stirred at a second stirring speed.
[0016] In the method for preparing the ceramic micro-nano fiber aerogel material, the first stirring speed is 400-800 rpm; the first stirring time is 6-8 hours;
[0017] The second stirring speed is 400-1200 rpm; the second stirring time is 5-24 hours.
[0018] In the method for preparing the ceramic micro-nano fiber aerogel material, in the step of preparing the precursor, the relative humidity of the spinning environment is 20-30%.
[0019] In the method for preparing the ceramic micro-nano fiber aerogel material, the polymer is selected from at least one of polyvinyl alcohol, polyvinyl pyrrolidone and polyethylene oxide;
[0020] The solvent comprises at least one of water, formic acid, tetrahydrofuran, acetone, acetylacetone, butanone, n-hexane, cyclohexane, n-heptane, acetonitrile, N-methylpyrrolidone, 1,2-propylene glycol, chloroform, dichloromethane, 1,2-dichloroethane, methanol, ethanol, isopropanol, 1-methoxy-2-propanol, tert-butanol, n-butanol, n-propanol, toluene, xylene, ethylenediamine, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and carbon tetrachloride;
[0021] The catalyst includes at least one of hydrochloric acid, phosphoric acid, acetic acid and citric acid.
[0022] The present invention provides a ceramic micro-nano fiber aerogel material, and the ceramic micro-nano fiber aerogel material is prepared according to the above-mentioned preparation method.
[0023] The present invention provides an application of the above-mentioned ceramic micro-nano fiber aerogel material as a thermal insulation sheet between battery cells, a thermal insulation pad between a battery module and a shell, or a thermal insulation barrier between the outside of a battery pack and a vehicle compartment.
[0024] A technical solution in the present invention can have the following beneficial effects:
[0025] The preparation method of the present invention introduces a second silicon source into the precursor solution, and in the preparation process, follows the specified order of placing the raw materials and the stirring speed of the stirrer to ensure that the first silicon source and the second silicon source can be fully and evenly hydrolyzed to obtain a stable non-Newtonian fluid precursor solution, effectively extending the precursor solution spinning window period, thereby avoiding the problem of frequent replacement of the precursor solution, and improving the production efficiency of the ceramic micro-nano fiber aerogel material. At the same time, the prepared ceramic micro-nano fiber aerogel material has a low fiber density, a finer fiber diameter, and a good thermal insulation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the appearance diagram of the sample of Example 1 of the present invention;
[0027] Figure 2 This is a sample appearance diagram of Example 4 of the present invention;
[0028] Figure 3 This is a sample appearance diagram of Example 6 of the present invention;
[0029] Figure 4 This is the appearance diagram of the sample of Example 7 of the present invention;
[0030] Figure 5 This is a sample appearance diagram of Example 5 of the present invention;
[0031] Figure 6 This is a sample appearance diagram of Example 9 of the present invention;
[0032] Figure 7 It is a density analysis result diagram of Example 1, Example 4 and Example 6 of the present invention;
[0033] Figure 8 1 is a fiber diameter analysis diagram of Example 1, Example 4 and Example 6 of the present invention;
[0034] Fig. 9 is a SEM image of Example 5 of the present invention;
[0035] Fig.10 This is a SEM image of a single fiber of Example 5 of the present invention. DETAILED DESCRIPTION
[0036] The technical scheme of the present invention is further illustrated by specific embodiments below. In order to facilitate understanding of the present invention, the present invention is described more comprehensively below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0037] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0039] Please refer to Figures 1 to 10 The present invention provides a method for preparing a ceramic micro-nano fiber aerogel material, wherein the ceramic micro-nano fiber aerogel material is prepared from a precursor solution, wherein the precursor solution comprises a polymer, a first silicon source, a second silicon source and a catalyst; the second silicon source comprises one of a silane having three oxygen groups and a silane having two oxygen groups; the preparation method comprises the following steps:
[0040] Prepare a polymer solution: dissolve the polymer in a solvent, and stir at a first stirring speed for a first stirring time until the solution is uniform to form a polymer solution;
[0041] Preparing a precursor solution: adding a first silicon source and a second silicon source to a polymer solution, stirring at a second stirring speed, adding a catalyst dropwise during the stirring process, and standing after a second stirring time to obtain a precursor solution;
[0042] Preparing a precursor: spinning a spinnable precursor solution into solid micro-nano fibers using a spinning device, and the micro-nano fibers are accumulated on a collecting device to form fibers, thereby obtaining a ceramic micro-nano fiber aerogel precursor;
[0043] Sintering precursor: putting the ceramic micro-nano fiber aerogel precursor into a boiler for sintering, the sintering temperature is 950-1100° C., the sintering time is 0.8-1.2 hours, and the ceramic micro-nano fiber aerogel material is obtained by sintering.
[0044] The preparation method of the present invention introduces a second silicon source into the precursor solution, and in the preparation process, follows the specified order of placing the raw materials and the stirring speed of the stirrer to ensure that the first silicon source and the second silicon source can be fully and evenly hydrolyzed to obtain a stable non-Newtonian fluid precursor solution, effectively extending the precursor solution spinning window period, thereby avoiding the problem of frequent replacement of the precursor solution, and improving the production efficiency of the ceramic micro-nano fiber aerogel material. At the same time, the prepared ceramic micro-nano fiber aerogel material has a low fiber density, a finer fiber diameter, and a good thermal insulation effect.
[0045] The spinning device is a centrifugal spinning device or a centrifugal electrostatic spinning device, and the specific spinning process of the spinning device includes:
[0046] Loading the precursor solution: When the ambient humidity inside the centrifugal spinning machine drops to about 30%, turn on the power to start the equipment, the spinning disk starts to rotate driven by the motor, set the speed of the spinning disk to 200rpm, load the precursor solution into the liquid storage tank, and spread the precursor solution evenly in the liquid storage tank;
[0047] Fiber formation and collection: After loading the precursor solution, adjust the speed of the spinning disk to 4000rpm, and the spinning disk rotates at high speed. If the precursor solution remains spinnable, the precursor solution will be ejected from the needle of the spinning disk and stretched into filaments in the air, and then air-dried at room temperature and pressure to form fibers. Under the action of the wind from the fan above, the fibers are collected on the collection net; if the precursor solution loses its spinnability, no fibers will be generated.
[0048] In the step of sintering the precursor, the boiler is heated from 20°C to 1000°C at a rate of 5°C / min, kept warm for 1 hour, and then naturally cooled to room temperature to obtain the ceramic micro-nano fiber aerogel material.
[0049] Specifically, the first silicon source is tetraethyl silicate, and the second silicon source includes one of 3-aminopropyltrimethoxysilane (APMTS), γ-glycidyloxypropyltrimethoxysilane (GPTMS), dimethyldimethoxysilane (DMDMS) and methyltrimethoxysilane (MTMS).
[0050] The second silicon source and tetraethyl silicate are both silicates, which are chemically compatible and can be hydrolyzed and polycondensed together in the same solution, so that the PVP / TEOS / GPTMS system remains stable. Moreover, the addition of the second silicon source changes the concentration and distribution of silicate groups in the system, and the hydroxyl groups produced by the hydrolysis of the second silicon source itself also participate in the condensation reaction, thereby affecting the formation rate of silicon-oxygen bonds (-Si-O-Si-), slowing down the progress of the condensation reaction, and helping to slowly and evenly promote the polycondensation reaction, thereby avoiding premature gelation or excessive solution viscosity, which is conducive to maintaining good spinning conditions.
[0051] In a preferred embodiment, (3-glycidyl propoxy) trimethoxy silane is used as the second silicon source. The amino group of (3-glycidyl propoxy) trimethoxy silane interacts with the carboxyl or ketone group of the polymer to form a more stable polymer network, maintain the structural integrity and stable rheological properties of the solution, and form a structure in which the silane coupling agent wraps TEOS, so that the hydrolysis of TEOS becomes slow. In combination with gentle stirring, the structural integrity and stable rheological properties of the solution are maintained, thereby extending the spinning window period of the precursor solution.
[0052] In addition, (3-glycidyl propoxy) trimethoxysilane can adjust the viscosity and reaction rate. The methoxy group (-OMe) in (3-glycidyl propoxy) trimethoxysilane undergoes a hydrolysis reaction in the solution system to form a hydroxyl group (-OH). The hydrolysis reaction rate of (3-glycidyl propoxy) trimethoxysilane is slower than that of tetraethyl silicate. Therefore, in the whole system, the addition of (3-glycidyl propoxy) trimethoxysilane can slow down the overall hydrolysis and polycondensation rate, thereby helping to extend the spinning window period of the solution.
[0053] Specifically, the concentration of the polymer is 0.0007-0.0013 mol / L; the concentration of the first silicon source is 0.96-1.20 mol / L; the concentration of the second silicon source is 0.18-0.48 mol / L; and the concentration of the catalyst is 0.15-0.25 mol / L.
[0054] By adopting the above concentration, the hydrolysis rate of the first silicon source is appropriately slowed down while ensuring the smooth hydrolysis of the first silicon source, thereby extending the spinnable time of the precursor solution. The molecular weight of PVP is 1 million. In a specific embodiment of the present invention, the polymer solution is obtained by mixing 15g of PVP powder with 85g of deionized water, and the mass fraction of the PVP solution is calculated to be 15%.
[0055] Preferably, the molar ratio of the first silicon source to the second silicon source is 7:1 to 1:1. With the above concentration, the stability of the precursor solution system is ensured while ensuring that the prepared ceramic micro-nano fiber aerogel material is more fluffy.
[0056] Specifically, in the step of preparing the precursor solution, the polymer solution is placed in an environment of 25-40° C. and stirred at a second stirring speed.
[0057] Since the hydrolysis and polycondensation rates of tetraethyl silicate and (3-glycidyl propoxy) trimethoxysilane are faster at high temperatures, if the temperature in the step of preparing the precursor solution is higher than 40° C., the spinning window period of the precursor solution will be shortened. In a specific embodiment of the present invention, the step of preparing the precursor solution is carried out in a constant temperature water bath stirrer, and the catalyst is gradually added dropwise.
[0058] Specifically, the first stirring speed is 400-800 rpm; the first stirring time is 6-8 hours;
[0059] The second stirring speed is 400-1200 rpm; the second stirring time is 5-24 hours.
[0060] The purpose of the first stirring process of preparing the polymer solution is to disperse the polymer so that the polymer is more evenly distributed in the solution. The purpose of the second stirring process of preparing the precursor solution is to disperse the first silicon source, the second silicon source and the catalyst, improve the uniformity of the first silicon source, the second silicon source and the catalyst in the solution, make the hydrolysis and polycondensation reactions of the first silicon source and the second silicon source more thorough, and tend to form a more uniform and slightly loose three-dimensional network structure. These network structures help to form large-pore and low-density materials in the subsequent drying or heat treatment process. Therefore, the longer the stirring time of preparing the precursor solution, the fluffier the obtained fiber.
[0061] However, when the stirring time of the second stirring process of the precursor solution is greater than 24 hours, the fibers become rough and there are a large number of droplets on the fiber surface. The droplets increase the adhesion between the fibers, causing the fiber bundles to easily aggregate and entangle, which may affect the mechanical properties of the material, such as elasticity and tensile strength. Therefore, too long a stirring time is not conducive to the formation of uniform SiO2 fiber aerogels, and the spinning effect will deteriorate instead.
[0062] Specifically, in the step of preparing the precursor, the relative humidity of the spinning environment is 20-30%.
[0063] The relative humidity is controlled at 20-35%, and the obtained fiber is dry and fluffy, which is easy to collect. If the humidity of the spinning environment is too high, the fiber drying speed will be slowed down, there will be more droplets on the fiber membrane surface, and then the fiber will stick together, which is not conducive to collecting fluffy fibers.
[0064] Specifically, the polymer is selected from at least one of polyvinyl alcohol, polyvinyl pyrrolidone and polyethylene oxide;
[0065] The solvent comprises at least one of water, formic acid, tetrahydrofuran, acetone, acetylacetone, butanone, n-hexane, cyclohexane, n-heptane, acetonitrile, N-methylpyrrolidone, 1,2-propylene glycol, chloroform, dichloromethane, 1,2-dichloroethane, methanol, ethanol, isopropanol, 1-methoxy-2-propanol, tert-butanol, n-butanol, n-propanol, toluene, xylene, ethylenediamine, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and carbon tetrachloride;
[0066] The catalyst includes at least one of hydrochloric acid, phosphoric acid, acetic acid and citric acid.
[0067] The raw materials of polyvinyl alcohol are relatively cheap, and the production process is relatively mature, so the cost of large-scale production is relatively low. However, PVP has high thermal stability, can be spun and heat-treated at relatively high temperatures, and is not easy to decompose, while polyvinyl alcohol has relatively low thermal stability and is easy to decompose under high temperature conditions. In addition, polyvinyl alcohol has a certain degree of hygroscopicity and easily absorbs moisture in the environment, which may affect the application of ceramic micro-nano fiber aerogel materials in humidity-sensitive environments.
[0068] Polyethylene oxide has low toxicity, high tensile properties, and can form thin and continuous fibers, making it suitable for preparing nanofibers. However, compared with polyvinyl pyrrolidone, polyethylene oxide has poor thermal stability and relatively low mechanical strength.
[0069] The type of catalyst will affect the hydrolysis and polycondensation reaction rates. The hydrolysis reaction rate is faster under acid catalysis, and the hydrolysis reaction rate is slower under base catalysis; in the specific embodiment of the present invention, an acidic catalyst is used.
[0070] In some specific embodiments of the present invention, the solvent used is water, the polymer is one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), polyethylene oxide (PEO) and the like; and the catalyst is phosphoric acid, referred to as PA.
[0071] The present invention also provides a ceramic micro-nano fiber aerogel material, and the ceramic micro-nano fiber aerogel material is prepared according to the above-mentioned preparation method.
[0072] The ceramic micro-nano fiber aerogel material prepared by the above method has the characteristics of fluffy fibers, that is, low fiber density and finer fiber diameter, and has heat insulation and thermal insulation functions.
[0073] The present invention also provides an application of the above-mentioned ceramic micro-nano fiber aerogel material as a thermal insulation sheet between battery cells, a thermal insulation pad between a battery module and a shell, or a thermal insulation barrier between the outside of a battery pack and a vehicle compartment.
[0074] The ceramic micro-nano fiber aerogel material obtained by the above preparation method has excellent thermal insulation performance and chemical stability, and can be used between battery cells, between battery modules and shells, or between the outside of the battery pack and the vehicle to achieve the purpose of thermal insulation, prevent heat conduction and maintain the internal temperature of the battery stable, thereby providing safety and stability for new energy vehicles.
[0075] Example Group
[0076] A method for preparing a ceramic micro-nano fiber aerogel material, the preparation method comprising the following steps:
[0077] Prepare a polymer solution: dissolve the polymer in a solvent according to the proportions in Table 1, and stir at a first stirring speed for a first stirring time until the solution is uniform to form a polymer solution;
[0078] Prepare a precursor solution: add the first silicon source and the second silicon source to the polymer solution according to the ratio in Table 1, stir at a second stirring speed, add a catalyst dropwise during the stirring process, and stand for the second stirring time to obtain a precursor solution;
[0079] Preparing a precursor: spinning a spinnable precursor solution into solid micro-nano fibers using a spinning device, and the micro-nano fibers are accumulated on a collecting device to form fibers, thereby obtaining a ceramic micro-nano fiber aerogel precursor;
[0080] Sintering precursor: Place the ceramic micro-nano fiber aerogel precursor in a muffle furnace for sintering, raise the temperature from 20°C to 1000°C at a rate of 5°C / min, keep the temperature for 1 hour, and sinter to obtain the ceramic micro-nano fiber aerogel material.
[0081] Table 1- Precursor solution ratio and preparation parameters
[0082]
[0083] The first stirring speed is 500 rpm, the second stirring speed is 800 rpm, the relative humidity of the spinning environment is 30%, the first silicon source is tetraethyl silicate, the second silicon source is (3-glycidyl propoxy) trimethoxy silane, the solvent used is water, the polymer in Examples 1 to 14 is polyvinyl pyrrolidone, the polymer in Examples 15 to 17 is polyethylene oxide, and the polymer in Examples 18 to 20 is polyethyl alcohol, and the catalyst is phosphoric acid.
[0084] In addition, the precursor solutions in Example 10 and Examples 12 to 14 have a high viscosity and have lost fluidity and are in a gel state. After being prepared, they cannot be spun.
[0085] Embodiment 21
[0086] The preparation method and components of Example 21 are the same as those of Example 1, except that the relative humidity of the spinning environment is 40%.
[0087] The ceramic micro-nano fiber aerogel materials obtained by sintering Examples 1 to 21 were observed for appearance to determine the state of the fibers, and density analysis was performed on Examples 1, 4, and 6, that is, the obtained ceramic micro-nano fiber aerogel materials were cut into regular blocks, and their length, width, and height were measured with a vernier caliper to calculate their volume, and then their mass was measured with a balance to obtain the density of the fibers; the fiber diameters were analyzed with a scanning electron microscope, and the density analysis results are shown in FIG. Figure 7 , fiber diameter analysis results are shown in Figure 8 The fiber state of Example 5 was better than that of Example 5, and a scanning electron microscope was used for observation.
[0088] Among them, Examples 15 to 20 are spinning experiments performed by replacing the polymer solution, wherein in Examples 15 to 17, the polymer selected is polyethylene oxide, the spinning state is good, and the fiber state is dry and fluffy; in Examples 18 to 20, the polymer selected is polyethyl alcohol, the spinning state is good, and the fiber is easy to absorb moisture and stick together.
[0089] By comparing Example 1, Example 4 and Example 6, it can be seen that the higher the molar ratio of the first silicon source to the second silicon source, the better the stability of the system. However, since the organic functional groups in the second silicon source, such as epoxy groups, can cause more chemical crosslinking, it is not conducive to the preparation of fluffy SiO2 fibers.
[0090] Comparing Example 6 and Example 7, it can be seen that the higher the stirring temperature, the faster the hydrolysis and polycondensation of tetraethyl silicate and (3-glycidyl propoxy) trimethoxy silane, and the worse the stability of the system. Properly extending the stirring time is conducive to obtaining SiO2 fibers with lower density and finer fiber diameter, but when the stirring time is too long, the fiber diameter and density will increase, and a large number of droplets will appear on the fiber surface, affecting its mechanical properties.
[0091] according to Figure 7 It can be seen that the density of the obtained fiber increases with the increase of the second silicon source content, because the second silicon source forms a siloxane network structure after hydrolysis. A higher content of the second silicon source means the formation of more crosslinking points, thereby increasing the density of the network structure and thus increasing the overall density of the fiber; moreover, the second silicon source is easy to form a more complex network structure through condensation reaction through its functional groups. As the content of the second silicon source increases, the condensation reaction is more thorough, the three-dimensional network structure formed is tighter, and the density of the fiber increases accordingly.
[0092] When the stirring time was extended from 5h to 10h, the fiber diameter decreased slightly. After stirring for 5 hours, due to insufficient stirring time, the hydrolysis and polycondensation reactions of the first and second silicon sources in the solution may not be sufficient, the PVP is not fully disentangled and dispersed, the viscosity of the precursor solution is low, and it cannot be effectively stretched into fine fibers, thus forming a coarse fiber structure. With the increase of stirring time, the hydrolysis and polycondensation of the first and second silicon sources are more sufficient, the PVP molecules are better disentangled and dispersed, the uniformity of the solution viscosity is improved, and finally the fiber diameter is optimized.
[0093] When the stirring time is extended from 10h to 24h, the fiber diameter increases. The reason is speculated to be that the longer stirring time allows the precursors to be fully mixed, the polycondensation reaction time is long, and larger siloxane (Si-O-Si) aggregates are formed, thus forming thicker fibers; and, as the stirring time increases, the polymers in the solution may aggregate, increasing the viscosity of the solution through self-entanglement and mutual physical entanglement. Higher solution viscosity will lead to thicker fiber formation during the spinning process.
[0094] When collecting the ceramic micro-nano fiber aerogel precursor of Example 15, compared with Example 1, the humidity in Example 15 is too high, resulting in a slower fiber drying speed, more droplets on the fiber membrane surface, and then fiber adhesion, which is not conducive to collecting fluffy fibers.
[0095] pass Fig.10 It can be obtained that the diameter of the ceramic micro-nano fiber aerogel material is about 1.4μm. By comparing the diameter of the SiO2 fiber produced by the PVP / TEOS system with the diameter of the SiO2 fiber produced by the PVP / TEOS / GPTMS system, it can be found that after adding GPTMS, the fiber diameter is smaller under appropriate stirring time, which is conducive to the preparation of aerogel materials with lower thermal conductivity.
[0096] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific embodiments of the present invention without creative work, and these equivalent variations or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for preparing a ceramic micro-nano fiber aerogel material, characterized in that: The ceramic micro-nano fiber aerogel material is prepared from a precursor solution, wherein the precursor solution comprises a polymer, a first silicon source, a second silicon source and a catalyst; the second silicon source comprises one of a silane having three oxygen groups and a silane having two oxygen groups; the preparation method comprises the following steps: Prepare a polymer solution: dissolve the polymer in a solvent, and stir at a first stirring speed for a first stirring time until the solution is uniform to form a polymer solution; Preparing a precursor solution: adding a first silicon source and a second silicon source to a polymer solution, stirring at a second stirring speed, adding a catalyst dropwise during the stirring process, and standing after a second stirring time to obtain a precursor solution; Preparing a precursor: spinning a spinnable precursor solution into solid micro-nano fibers using a spinning device, and the micro-nano fibers are accumulated on a collecting device to form fibers, thereby obtaining a ceramic micro-nano fiber aerogel precursor; Sintering precursor: putting the ceramic micro-nano fiber aerogel precursor into a boiler for sintering, the sintering temperature is 950-1100° C., the sintering time is 0.8-1.2 hours, and the ceramic micro-nano fiber aerogel material is obtained by sintering.
2. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: The first silicon source is tetraethyl silicate, and the second silicon source includes one of 3-aminopropyltrimethoxysilane (APMTS), γ-glycidyloxypropyltrimethoxysilane (GPTMS), dimethyldimethoxysilane (DMDMS) and methyltrimethoxysilane (MTMS).
3. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: The concentration of the polymer is 0.0007-0.0013 mol / L; the concentration of the first silicon source is 0.96-1.20 mol / L; the concentration of the second silicon source is 0.18-0.48 mol / L; and the concentration of the catalyst is 0.15-0.25 mol / L.
4. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: The molar ratio of the first silicon source to the second silicon source is 7:1 to 1:
1.
5. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: In the step of preparing the precursor solution, the polymer solution is placed in an environment of 25-65° C. and stirred at a second stirring speed.
6. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: The first stirring speed is 400-800 rpm; the first stirring time is 6-8 hours; The second stirring speed is 400-1200 rpm; the second stirring time is 5-24 hours.
7. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: In the step of preparing the precursor, the relative humidity is 20-45%.
8. The method for preparing a ceramic micro-nano fiber aerogel material according to claim 1, characterized in that: The polymer is selected from at least one of polyvinyl alcohol, polyvinyl pyrrolidone and polyethylene oxide; The solvent comprises at least one of water, formic acid, tetrahydrofuran, acetone, acetylacetone, butanone, n-hexane, cyclohexane, n-heptane, acetonitrile, N-methylpyrrolidone, 1,2-propylene glycol, chloroform, dichloromethane, 1,2-dichloroethane, methanol, ethanol, isopropanol, 1-methoxy-2-propanol, tert-butanol, n-butanol, n-propanol, toluene, xylene, ethylenediamine, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and carbon tetrachloride; The catalyst includes at least one of hydrochloric acid, phosphoric acid, acetic acid and citric acid.
9. A ceramic micro-nano fiber aerogel material, characterized in that: The ceramic micro-nano fiber aerogel material is prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the ceramic micro-nano fiber aerogel material according to claim 9 as a thermal insulation sheet between battery cells, a thermal insulation pad between a battery module and a shell, or a thermal insulation barrier between the outside of a battery pack and a vehicle compartment.
Citation Information
Patent Citations
Silica nanoscale hybridized sol thermochromatic finishing method for fabric
CN102345231A
Preparation method of silicon-carbide-fibrofelt-enhanced silica aerogel composite material
CN103360019A
Heat-insulating and high-temperature-resistant aerogel gradient composite material and preparation method thereof
CN112830760A
Preparation method and application of OPUSA composite aerogel
CN113831583A
Silicon electrode material with good cycling stability and preparation method thereof
CN115057443A