Rapid reaction type self-healing microcapsule material for recycled asphalt mixture and preparation method of rapid reaction type self-healing microcapsule material

By using fast-reactive self-healing microcapsule materials in regenerated asphalt and chemical grafting reaction of crosslinking agents with aged SBS, the problem of vulnerability to the pavement of regenerated asphalt has been solved, and its rapid self-healing and performance improvement has been achieved. Extend service life.

CN118925611APending Publication Date: 2024-11-12HOHAI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411064124.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Recycled asphalt pavement is prone to cracks and damage during use, resulting in a degradation of its road performance and shortening its service life, and it is difficult for the existing technology to repair quickly and efficiently.

Method used

Using fast-reacting self-healing microcapsules material, microcapsules that can self-heal in regenerated asphalt are prepared by mixing regenerated agents, crosslinking agents and penetrants with resins and modifiers, adjusting pH values ​​and heating reactions. Materials, chemical grafting reaction is performed with the end groups of aged SBS using crosslinking agents to reconstruct the molecular structure and improve the elastic characteristics of asphalt.

Benefits of technology

It achieves rapid and efficient self-healing of regenerated asphalt, extends the service life of regenerated asphalt pavement, and accelerates the regeneration of aged asphalt through penetrants, improving road performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925611A_ABST
    Figure CN118925611A_ABST
Patent Text Reader

Abstract

The invention discloses a rapid reaction type self-healing microcapsule material for a recycled asphalt mixture and a preparation method of the rapid reaction type self-healing microcapsule material, and belongs to the technical field of highway engineering materials. The preparation method of the rapid reaction type self-healing microcapsule material for the recycled asphalt mixture comprises the following steps: adding a regenerant, a cross-linking agent and a penetrant into water, and mixing and emulsifying to obtain an emulsion; adding resin and a modifier into the emulsion, adjusting the pH value to be acidic, and heating for reaction to obtain a suspension; and centrifuging and drying the suspension to obtain the rapid reaction type self-healing microcapsule material. The rapid reaction type self-healing microcapsule material provided by the invention can rapidly and efficiently promote the self-healing of the recycled asphalt and improve the pavement performance of the recycled asphalt so as to prolong the service life of the recycled asphalt pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of highway engineering materials, and in particular to a fast-response self-healing microcapsule material for regenerating asphalt mixture and a preparation method thereof. Background Art

[0002] Asphalt pavement has excellent road performance, but it will age over time and needs regular maintenance. Following the concept of green maintenance, environmental pollution and resource waste should be reduced at all stages of asphalt pavement construction. Traditional milling and resurfacing methods consume and emit a large amount of non-renewable resources. By adopting recycling technology and using waste asphalt pavement materials to resurface new pavement, it is possible to save resources, reduce costs, and improve efficiency.

[0003] Fatigue damage of asphalt pavement can be attributed to the initiation and expansion of internal cracks in asphalt pavement under repeated loads. When these cracks or damages cannot be repaired and treated in a timely and effective manner, macro cracks will occur and lead to structural brittle fractures. Recycled asphalt mixtures are made from aged asphalt in old asphalt pavement materials. Their fatigue cracking performance is often worse than that of new materials. Cracks or damage will inevitably occur during use, affecting the road performance and service life of asphalt pavement. For this reason, there is an urgent need for a method or technology that can quickly and efficiently repair tiny cracks and damaged areas in recycled modified asphalt pavement, thereby improving the road performance of recycled modified asphalt pavement and extending the service life of recycled asphalt pavement. Summary of the invention

[0004] The purpose of the present invention is to provide a fast-response self-healing microcapsule material for regenerated asphalt mixture and a preparation method thereof to solve the problems existing in the above-mentioned prior art. The fast-response self-healing microcapsule material of the present invention can quickly and efficiently promote the self-healing of regenerated asphalt, improve the road performance of regenerated asphalt and extend the service life of the regenerated asphalt pavement.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention: a method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture, comprising the following steps:

[0007] Adding a regenerating agent, a cross-linking agent and a penetrant into water, mixing and emulsifying to obtain an emulsion;

[0008] Adding resin and modifier into the emulsion, adjusting the pH value to acidic, heating for reaction, and obtaining a suspension;

[0009] The suspension is centrifuged and dried to obtain the rapid-response self-healing microcapsule material.

[0010] Further, the regeneration agent includes any one of a mixture of dibutyl phthalate and dioctyl phthalate, aromatic oil, C9 petroleum resin and sorbitan fatty acid ester;

[0011] The cross-linking agent includes a diisocyanate prepolymer;

[0012] The penetrant includes polyoxyethylene isooctyl alcohol ether or polyoxyethylene isooctyl alcohol ether phosphate.

[0013] Furthermore, the method for preparing the dibasic isocyanate prepolymer comprises the following steps:

[0014] The vacuum dehydrated terminal hydroxyl oligomer is heated to 70-80° C., and then a diisocyanate compound is added, and the mixture is stirred and reacted for 2-3 hours under a nitrogen environment to obtain the diisocyanate prepolymer.

[0015] Furthermore, the mixing and emulsification method specifically includes: shearing emulsification at a shear rate of 3500 r / min for 30 min, then heating to 160-180° C., and then stirring at a stirring rate of 500-800 r / min for 1 h;

[0016] The pH value of the system during the mixed emulsification is neutral.

[0017] Further, the resin includes any one of polymethyl methacrylate resin, polymelamine formaldehyde resin and melamine urea formaldehyde resin;

[0018] The modifier includes a silane coupling agent.

[0019] Furthermore, the silane coupling agent includes any one of γ-aminotriethoxysilane, silane coupling agent KH-560 and silane coupling agent KH-570.

[0020] Further, the ratio of the total mass of the resin and the modifier to the total mass of the regeneration agent, the cross-linking agent and the penetrant is 5:6;

[0021] The mass ratio of the resin to the modifier is 100:(3-5);

[0022] The mass percentages of the regeneration agent, the cross-linking agent and the penetrant are 60-80%: 15-20%: 5%-10%, and the total is 100%.

[0023] Furthermore, the pH value is adjusted to acidity to adjust the pH value to 3.5-4; and the temperature of the heating reaction is 60-70°C.

[0024] The second technical solution of the present invention: a fast-response self-healing microcapsule material prepared by the above-mentioned preparation method.

[0025] The third technical solution of the present invention: an application of the above-mentioned fast-response self-healing microcapsule material in the preparation of regenerated asphalt pavement.

[0026] The present invention discloses the following technical effects:

[0027] (1) The preparation method of the fast-response self-healing microcapsule material of the present invention is simpler, easier to operate, and has better performance.

[0028] (2) The fast-response self-healing microcapsule material of the present invention can quickly and efficiently promote the self-healing of regenerated asphalt, improve the road performance of regenerated asphalt and extend the service life of the regenerated asphalt pavement.

[0029] (3) The penetrant contained in the fast-response self-healing microcapsule material of the present invention can accelerate the diffusion rate of the microcapsule material in aged asphalt (aged asphalt contained in the regenerated asphalt) and improve the regeneration degree of the aged asphalt; the cross-linking agent (diisocyanate prepolymer) contained in the material is a reactive difunctional compound, which can undergo a chemical grafting reaction with the end groups of the aged degradation products of SBS to reconstruct the molecular structure of SBS, thereby allowing the aged SBS to regain the characteristics of an elastomeric body. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a physical picture of the fast-response self-healing microcapsule material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] In a first aspect, the present invention provides a method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture, comprising the following steps:

[0038] Adding a regenerating agent, a cross-linking agent and a penetrant into water, mixing and emulsifying to obtain an emulsion;

[0039] Adding resin and modifier into the emulsion, adjusting the pH value to acidic, heating for reaction, and obtaining a suspension;

[0040] The suspension is centrifuged and dried to obtain a fast-response self-healing microcapsule material.

[0041] The regeneration agent used in the present invention comprises any one of a mixture of dibutyl phthalate and dioctyl phthalate (the mass ratio of dibutyl phthalate to dioctyl phthalate is 1:1), aromatic oil (perilla aromatic oil), C9 petroleum resin and sorbitan fatty acid ester; the crosslinking agent comprises a diisocyanate prepolymer; and the penetrant comprises polyoxyethylene isooctyl alcohol ether or polyoxyethylene isooctyl alcohol ether phosphate.

[0042] The method for preparing the diisocyanate prepolymer comprises the following steps:

[0043] The vacuum dehydrated terminal hydroxyl oligomer (terminal hydroxyl butadiene with a number average molecular weight of 2500-2800) is heated to 70-80° C., and then a diisocyanate compound is added, and the mixture is stirred and reacted for 2h-3h under a nitrogen environment to obtain a diisocyanate prepolymer.

[0044] The mixed emulsification method adopted by the present invention specifically includes: shearing emulsification at a shear speed of 3500r / min for 30min, then heating to 160-180°C, and then stirring at a stirring speed of 500-800r / min for 1h; the pH value of the system is neutral during the mixed emulsification.

[0045] The resin used in the present invention includes any one of polymethyl methacrylate resin (Zhenjiang Chimei CM-205), polyurethane acrylate (Hubei Kewode RJ4247) and melamine urea-formaldehyde resin (Funneng);

[0046] The modifier used in the present invention includes a silane coupling agent; the silane coupling agent includes any one of gamma-aminotriethoxysilane, silane coupling agent KH-560 and silane coupling agent KH-570.

[0047] In the present invention, the ratio of the total mass of the resin and the modifier to the total mass of the regeneration agent, the crosslinking agent and the penetrant is 5:6; the mass ratio of the resin and the modifier is 100:(3-5); the mass percentages of the regeneration agent, the crosslinking agent and the penetrant are 60-80%:15-20%:5%-10%, and the total is 100%.

[0048] In the present invention, adjusting the pH value to acidic is adjusting the pH value to 3.5-4; and the temperature of the heating reaction is 60-70°C.

[0049] The second aspect of the present invention provides a fast-response self-healing microcapsule material prepared by the above preparation method.

[0050] The third aspect of the present invention provides an application of the above-mentioned fast-response self-healing microcapsule material in the preparation of regenerated asphalt pavement.

[0051] Example 1

[0052] A method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture:

[0053] (1) The fast-response self-healing microcapsule material is composed of a capsule wall and a capsule core, and the mass ratio of the capsule wall raw material to the capsule core raw material is 5:6, wherein the capsule wall raw material is a resin and a modifier in a mass ratio of 100:4 (the resin and the modifier react to form a modified resin), and the capsule core raw material is a regeneration agent, a cross-linking agent and a penetrant, and the mass percentages of the components of the capsule core raw material are: regeneration agent 70%, cross-linking agent 20%, and penetrant 10%.

[0054] The resin is polymethyl methacrylate resin (Zhenjiang Chimei CM-205); the modifier is γ-aminotriethoxysilane; the regeneration agent is a mixture of dibutyl phthalate and dioctyl phthalate (the mass ratio of dibutyl phthalate to dioctyl phthalate is 1:1); the crosslinking agent is a diisocyanate prepolymer; the penetrant is isooctyl alcohol polyoxyethylene ether;

[0055] The preparation method of the crosslinking agent is as follows: 10g of vacuum dehydrated terminal hydroxyl oligomer (terminal hydroxyl butadiene with a number average molecular weight of 2500-2800) is heated to 80°C, 4g of a diisocyanate compound is added, and the mixture is stirred and reacted for 3h under a nitrogen environment to obtain a diisocyanate prepolymer.

[0056] (2) Add the regeneration agent, cross-linking agent and penetrant into deionized water, adjust the pH to neutral with diluted hydrochloric acid, use a shear emulsifier to shear emulsify at a shear rate of 3500 r / min for 30 min (normal temperature), raise the temperature to 160°C, and stir at 500 r / min for 1 h with a stirrer to obtain a completely dissolved uniform emulsion.

[0057] (3) Under stirring conditions, resin and modifier are added to the uniform emulsion, the flow rate of dilute hydrochloric acid is controlled, the pH is slowly adjusted to 3.5, and the temperature is raised to 65°C. After the internal phase is volatilized, a suspension is obtained; the obtained suspension is centrifuged, washed, and dried to obtain a fast-response self-healing microcapsule material for regenerating asphalt mixture (see the actual picture) Figure 1 ), the capsule core of the material is composed of a regeneration agent, a cross-linking agent and a penetrant, and the capsule wall is a modified resin generated by the reaction of a resin and a modifier.

[0058] Example 2

[0059] A method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture:

[0060] (1) The fast-response self-healing microcapsule material is composed of a capsule wall and a capsule core, and the mass ratio of the capsule wall material to the capsule core material is 5:6, wherein the capsule wall material is a resin and a modifier in a mass ratio of 100:5 (the resin and the modifier react to form a modified resin), and the capsule core material is a regeneration agent, a cross-linking agent and a penetrant, and the mass percentages of the components of the capsule core material are: regeneration agent 75%, cross-linking agent 15%, and penetrant 10%.

[0061] The resin is polyurethane acrylate (Hubei Kewode RJ4247); the modifier is silane coupling agent KH-560; the regeneration agent is perilla aromatic oil; the crosslinking agent is diisocyanate prepolymer; the penetrant is isooctyl alcohol polyoxyethylene ether phosphate;

[0062] The preparation method of the cross-linking agent is as follows: 10g of vacuum dehydrated terminal hydroxyl oligomer (terminal hydroxyl butadiene with a number average molecular weight of 2500-2800) is heated to 75°C, 4g of a diisocyanate compound is added, and the mixture is stirred and reacted for 2.5h under a nitrogen environment to obtain a diisocyanate prepolymer.

[0063] (2) Add the regeneration agent, cross-linking agent and penetrant into deionized water, adjust the pH to neutral with diluted hydrochloric acid, use a shear emulsifier to shear emulsify at a shear rate of 3500 r / min for 30 min (normal temperature), raise the temperature to 170°C, and stir at 650 r / min for 1 h with a stirrer to obtain a completely dissolved uniform emulsion.

[0064] (3) Under stirring conditions, resin and modifier are added to the uniform emulsion, the flow rate of dilute hydrochloric acid is controlled, the pH value is slowly adjusted to 3.7, and the temperature is raised to 67°C. After the internal phase is volatilized, a suspension is obtained; the obtained suspension is centrifuged, washed, and dried to obtain a fast-response self-healing microcapsule material for regenerating asphalt mixture, wherein the capsule core of the material is composed of a regeneration agent, a cross-linking agent, and a penetrant, and the capsule wall is a modified resin generated by the reaction of the resin and the modifier.

[0065] Example 3

[0066] A method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture:

[0067] (1) The fast-response self-healing microcapsule material is composed of a capsule wall and a capsule core, and the mass ratio of the capsule wall material to the capsule core material is 5:6, wherein the capsule wall material is a resin and a modifier in a mass ratio of 100:3 (the resin and the modifier react to form a modified resin), and the capsule core material is a regeneration agent, a cross-linking agent and a penetrant, and the mass percentages of the components of the capsule core material are: regeneration agent 80, cross-linking agent 10%, and penetrant 10%.

[0068] The resin is melamine urea-formaldehyde resin (Funneng); the modifier is silane coupling agent KH-570; the regeneration agent is sorbitan fatty acid ester; the crosslinking agent is diisocyanate prepolymer; the penetrant is isooctyl alcohol polyoxyethylene ether;

[0069] The preparation method of the crosslinking agent is as follows: 10g of vacuum dehydrated terminal hydroxyl oligomer (terminal hydroxyl butadiene with a number average molecular weight of 2500-2800) is heated to 70°C, 4g of a diisocyanate compound is added, and the mixture is stirred and reacted for 2h under a nitrogen environment to obtain a diisocyanate prepolymer.

[0070] (2) Add the regeneration agent, cross-linking agent and penetrant into deionized water, adjust the pH to neutral with diluted hydrochloric acid, use a shear emulsifier to shear emulsify at a shear rate of 3500 r / min for 30 min (normal temperature), raise the temperature to 180°C, and stir at 800 r / min for 1 h with a stirrer to obtain a completely dissolved uniform emulsion.

[0071] (3) Under stirring conditions, resin and modifier are added to the uniform emulsion, the flow rate of dilute hydrochloric acid is controlled, the pH value is slowly adjusted to 4, and the temperature is raised to 70°C. After the internal phase is volatilized, a suspension is obtained; the obtained suspension is centrifuged, washed, and dried to obtain a fast-response self-healing microcapsule material for regenerating asphalt mixture, wherein the capsule core of the material is composed of a regeneration agent, a cross-linking agent, and a penetrant, and the capsule wall is a modified resin generated by the reaction of the resin and the modifier.

[0072] Comparative Example 1

[0073] Same as Example 1, except that no cross-linking agent is added.

[0074] Comparative Example 2

[0075] Same as Example 1, except that no penetrant is added.

[0076] Comparative Example 3

[0077] Same as Example 1, except that the resin is epoxy resin.

[0078] Comparative Example 4

[0079] The same as Example 1, except that the resin and the modifier are replaced with urea-formaldehyde prepolymer of equal mass.

[0080] Comparative Example 5

[0081] The same as Example 1, except that the cross-linking agent is a mixture of 1,4-butanediol diglycidyl ether and trimethylolpropane triglycidyl ether in a mass ratio of 4:1.

[0082] Comparative Example 6

[0083] The ratio of the total mass of urea and formaldehyde to the total mass of the regeneration agent, the surfactant and the defoaming agent is 2:3; the mass percentages of the regeneration agent, the surfactant and the defoaming agent are 90%, 8% and 2% respectively.

[0084] Pour urea and formaldehyde into a three-necked flask at a molar ratio of 4:5, adjust the pH to 9 with a diluted NaOH solution, and react in a water bath at 70°C for 60 minutes to obtain a urea-formaldehyde prepolymer; take 90% by weight of a regeneration agent, add an appropriate amount of deionized water and 8% by weight of a surfactant, use a rubber-tipped dropper to absorb a certain amount of diluted hydrochloric acid solution to adjust the pH to neutral, stir and disperse in a 50°C water bath for 20 minutes to obtain a stable asphalt regeneration agent oil emulsion; quickly transfer the emulsion to a three-necked flask, and slowly add the prepared urea-formaldehyde prepolymer into the three-necked flask, add 2% by weight of n-octane as a defoaming agent, control the flow rate of dilute hydrochloric acid, slowly adjust the solution pH to 4, heat to 70°C, and continue to react for 3 minutes after the reaction environment is stable; finally cool to room temperature, filter and wash the product, and vacuum dry to obtain microcapsules.

[0085] The performance of the microcapsules prepared in the examples and comparative examples was tested.

[0086] The recycled asphalt mixture adopts SMA-13 ​​grading, wherein RAP (recycled asphalt mixture) comes from the SMA-13 ​​upper layer of a certain expressway in Jiangsu, and the asphalt is SBS modified asphalt. The microcapsules (prepared in the embodiment and comparative example) are added when the asphalt mixture is mixed, and the added amount is 3% of the mass of the SBS modified asphalt. According to the standard of "Testing Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011), the recycled asphalt mixture plate specimens are formed by wheel rolling, and cut into small beam specimens with a length of 380 mm ± 5 mm, a thickness of 50 mm ± 5 mm, and a width of 63.5 mm ± 5 mm. The four-point bending test with strain control (400 με) is carried out to determine the fatigue life of the recycled asphalt mixture.

[0087] After the fatigue test, the specimen was placed in a 20°C environment for 48 hours, and then the specimen was subjected to the above-mentioned strain-controlled four-point bending test. The fatigue life recovery rate, i.e., the increased fatigue life after healing / the fatigue life before healing × 100%, was used to evaluate the self-healing effect of the recycled asphalt mixture.

[0088] Table 1 Self-healing effect

[0089]

[0090] It can be seen from Example 1 and Comparative Example 1 that the reactive cross-linking agent (diisocyanate prepolymer) has a significant effect on improving the self-repairing effect of the regenerated asphalt mixture; it can be seen from Example 1 and Example 3 that the reactive cross-linking agent (diisocyanate prepolymer) has an even more significant effect on improving the self-repairing effect than the regeneration agent, and the self-repairing effect of Example 1 is improved by 17.8% compared with Example 3; it can be seen from Example 1 and Comparative Example 2 that the penetrant has a significant effect on improving the self-repairing effect of the regenerated asphalt mixture, and the addition of the penetrant can achieve a rapid self-repairing effect of the regenerated asphalt mixture.

[0091] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a fast-response self-healing microcapsule material for regenerating asphalt mixture, characterized in that: The following steps are involved: Adding a regenerating agent, a cross-linking agent and a penetrant into water, mixing and emulsifying to obtain an emulsion; Adding resin and modifier into the emulsion, adjusting the pH value to acidic, heating for reaction, and obtaining a suspension; The suspension is centrifuged and dried to obtain the rapid-response self-healing microcapsule material.

2. The preparation method according to claim 1, characterized in that: The regeneration agent includes any one of a mixture of dibutyl phthalate and dioctyl phthalate, aromatic oil, C9 petroleum resin and sorbitan fatty acid ester; The cross-linking agent includes a diisocyanate prepolymer; The penetrant includes polyoxyethylene isooctyl alcohol ether or polyoxyethylene isooctyl alcohol ether phosphate.

3. The preparation method according to claim 2, characterized in that: The method for preparing the diisocyanate prepolymer comprises the following steps: The terminal hydroxyl oligomer is heated to 70-80° C., and then a diisocyanate compound is added thereto, and the mixture is stirred and reacted for 2-3 hours under a nitrogen environment to obtain the diisocyanate prepolymer.

4. The preparation method according to claim 1, characterized in that: The mixing and emulsification method specifically includes: shearing and emulsifying at a shear rate of 3500 r / min for 30 minutes, then heating to 160-180° C., and then stirring at a stirring rate of 500-800 r / min for 1 hour; The pH value of the system during the mixed emulsification is neutral.

5. The preparation method according to claim 1, characterized in that: The resin includes any one of polymethyl methacrylate resin, polymelamine formaldehyde resin and melamine urea formaldehyde resin; The modifier includes a silane coupling agent.

6. The preparation method according to claim 5, characterized in that: The silane coupling agent includes any one of γ-aminotriethoxysilane, silane coupling agent KH-560 and silane coupling agent KH-570.

7. The preparation method according to claim 1, characterized in that: The ratio of the total mass of the resin and the modifier to the total mass of the regeneration agent, the cross-linking agent and the penetrant is 5:6; The mass ratio of the resin to the modifier is 100:(3-5); The mass percentages of the regeneration agent, the cross-linking agent and the penetrant are 60-80%: 15-20%: 5%-10%, and the total is 100%.

8. The preparation method according to claim 1, characterized in that: The step of adjusting the pH value to acidic is adjusting the pH value to 3.5-4; and the temperature of the heating reaction is 60-70°C.

9. A fast-response self-healing microcapsule material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the fast-response self-healing microcapsule material according to claim 9 in the preparation of regenerated asphalt pavement.

Citation Information

Cited By

  • Production process of high-viscosity composite modified emulsified asphalt

    CN122541745A