Method for synthesizing heterogeneous silicate adsorption material by reconstructing coal gangue through plasma ball milling
Through plasma ball milling and heat treatment technology, coal gangue is converted into porous heterogeneous silicate adsorption materials, solving the problem of insufficient resource utilization in coal gangue solid waste treatment, and achieving efficient and environmentally friendly pollutant removal and environmental restoration.
Patent Information
- Application Number
- CN202410981288.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The pile of coal gangue solid waste occupies land, pollutes the environment, and the added value of existing treatment methods is not high. There is no effective technology to utilize its mineral and carbon components in all components, and high-value utilization has not been achieved.
The coal gangue was reconstructed by plasma ball mills and heat treatment, and porous heterogeneous silicate adsorption materials were prepared. The full-component conversion of coal gangue was achieved through pulverization, mixing, plasma ball milling and calcining under the protection of inert gas.
The prepared adsorbent materials have the ability to efficiently adsorb heavy metals, dyes and antibiotics, have stable product performance, and are convenient for industrial production, which realizes the resource utilization of coal gangue, avoids the emission of three wastes, and are suitable for water and soil pollution restoration.
Smart Images

Figure CN118925663A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue through plasma ball milling and synergistic heat treatment, belonging to the technical field of deep processing of natural non-metallic minerals and preparation of functional adsorption materials. Background Art
[0002] Gangue is a large solid waste generated in the process of coal production and coal washing, accounting for 15% of coal production. According to incomplete statistics, the cumulative amount of gangue in my country has exceeded 6 billion tons, and the emission is increasing year by year at a rate of about 500 million to 800 million tons per year. The huge amount of gangue solid waste not only occupies land and wastes resources, but also harms the ecological environment and human health, bringing serious environmental and safety hazards. At present, the main methods of disposing of gangue solid waste are backfilling, burying, stacking, paving roadbed, burning bricks, producing calcined kaolin, etc., but in general, the added value is not high, so the resource utilization of gangue has always received widespread attention, and new technologies for the resource utilization of gangue solid waste are urgently needed.
[0003] From a mineralogical point of view, coal gangue contains clay minerals represented by kaolinite (such as montmorillonite, illite, kaolinite, muscovite, quartz, feldspar, etc.), so coal gangue is also a natural mineral resource with abundant reserves. At the same time, coal gangue contains about 10-15% carbon, so coal gangue is also a natural carbon source. Taking advantage of the mineral properties of coal gangue, coal gangue can be directly calcined to produce calcined kaolin, and an industrial scale has been formed. However, during the calcination process, the carbon in the coal gangue will be converted into carbon dioxide emissions. Not only does it not take advantage of the inherent "carbon source" advantage of coal gangue, but carbon dioxide emissions also seriously pollute the environment. In addition, some researchers have also focused on extracting valuable components (such as aluminum) from coal gangue to improve its utilization rate, but because the alumina content in coal gangue is less than 50%, and it contains a variety of metal components, it is difficult to purify and separate, and the cost is high, so it is not economically feasible to use coal gangue to extract aluminum. Comprehensive analysis of the previous research results shows that the utilization of all components of minerals and carbon in coal gangue without the emission of three wastes is an inevitable trend to achieve high-value utilization of coal gangue. The present invention proposes a technical route for the coordinated transformation of minerals and activation of carbon components in coal gangue, and transforms coal gangue into porous silicate@carbon heterogeneous adsorption materials without introducing solvents and emitting three wastes. There are currently no reports and precedents for technical applications. Summary of the invention
[0004] The purpose of the present invention is to provide a method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue through plasma ball milling and synergistic heat treatment. The prepared material has an ultra-high adsorption capacity for heavy metals, dyes, antibiotics, etc., can coexist with the environment for a long time, and the preparation method is simple, which overcomes the shortcomings of existing adsorption materials. At the same time, it improves the added value of the comprehensive utilization of coal gangue with abundant reserves in the region.
[0005] The technical solution of the present invention is: the gangue is crushed and sieved to obtain the gangue powder, a certain mass of the gangue powder, alkali and oxidant are fully mixed, and then placed in a plasma ball mill, ground for 10-60 minutes, and then treated with plasma discharge for 10-120 seconds. The obtained product is calcined at 300-800°C for 1-6 hours under the protection of inert gas, and then cooled to room temperature to obtain the adsorption material.
[0006] In a possible implementation, the coal gangue is solid waste generated during coal mining or coal washing, wherein the content of inorganic non-metallic mineral components is 85% to 90%, and the carbon content is 10% to 15%.
[0007] In a possible implementation, the alkali is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, and potassium silicate.
[0008] In a possible implementation manner, the amount of the alkali used is 10% to 100% of the mass of the coal gangue.
[0009] In a possible implementation manner, the oxidant is one of hydrogen peroxide, potassium permanganate, ammonium persulfate, and potassium persulfate, and the amount used is 5% to 20% of the mass of the coal gangue.
[0010] In a possible implementation manner, the rotation speed of the ball mill is 100 to 1000 rpm, and the ball-to-material ratio is 1:1 to 3:1.
[0011] In a possible implementation manner, the radio frequency power of the plasma is 100-500 W, the frequency is 13.56 MHz, and the atmosphere is air.
[0012] In a possible implementation manner, the inert gas is one of nitrogen and argon, and the heating rate is 5-20° C. / min.
[0013] The present application provides a method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue through plasma ball milling, which has the following beneficial effects:
[0014] 1. Using coal gangue solid waste as raw material, porous silicate adsorption materials are prepared by direct full component conversion without complicated purification process. Coal gangue solid waste has abundant reserves, is economical and easy to obtain, green and non-toxic. The use of coal gangue to produce porous adsorption materials has achieved "turning waste into materials", which has economic and environmental benefits.
[0015] 2. The preparation process is simple and efficient, industrial production is convenient, no toxic or harmful reagents are used, no three wastes are discharged, and the product performance is stable.
[0016] 3. The product has high cost performance and is particularly suitable for the efficient removal of pollutants in water. It can also be used for the fixation of heavy metal pollutants in soil. It can be applied to many fields such as environmental remediation, deep water purification, and chemical product purification. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, without paying any creative work, other related drawings can be obtained based on these drawings and they also belong to the protection scope of the present application.
[0018] Figure 1 SEM images of (a) coal gangue powder and (b) heterogeneous silicate adsorption material (Si@C-1);
[0019] Figure 2 XRD patterns of coal gangue powder and heterogeneous silicate adsorption material (Si@C-1);
[0020] Figure 3 Raman spectrum of heterogeneous silicate adsorption material (Si@C-1). DETAILED DESCRIPTION
[0021] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below, and these embodiments cannot be interpreted as limiting the technical scheme. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0022] Embodiment 1:
[0023] Weigh 10 kg of coal gangue powder (inorganic non-metallic mineral component content 85%, carbon content 15%), mix it thoroughly with 1 kg of potassium hydroxide and 0.5 kg of potassium persulfate, and then place it in a plasma ball mill. Grind it for 10 minutes at a ball-to-material ratio of 1:1 and a rotation speed of 1000 rpm. Then treat it with plasma discharge (frequency of 13.56 MHz) at a radio frequency power of 100 W for 300 seconds. The obtained product is calcined at a heating rate of 20°C / min and a temperature of 800°C for 1 h under nitrogen gas protection. After cooling to room temperature, the adsorption material is obtained, which is marked as Si@C-1.
[0024] Embodiment 2:
[0025] Weigh 10 kg of coal gangue powder (inorganic non-metallic mineral component content 85%, carbon content 15%), mix it thoroughly with 10 kg of potassium carbonate and 0.5 kg of hydrogen peroxide, and then place it in a plasma ball mill, grind it for 60 minutes at a ball-to-material ratio of 3:1 and a rotation speed of 100 rpm, and then treat it with plasma discharge (frequency of 13.56 MHz) at a radio frequency power of 500 W for 20 seconds. The obtained product is calcined at a heating rate of 5 ° C / min and a temperature of 600 ° C under argon gas protection for 2 hours. After cooling to room temperature, the adsorption material is obtained, which is marked as Si@C-2.
[0026] Embodiment 3:
[0027] Weigh 10 kg of coal gangue powder (inorganic non-metallic mineral component content 90%, carbon content 10%), mix it thoroughly with 1 kg of potassium hydroxide, 0.2 kg of potassium carbonate and 2 kg of potassium permanganate, and then place it in a plasma ball mill, grind it for 30 minutes at a ball-to-material ratio of 1:1 and a rotation speed of 200 rpm, and then treat it with plasma discharge (frequency of 13.56 MHz) at a radio frequency power of 300 W for 80 seconds. The obtained product is calcined at a heating rate of 10°C / min and a temperature of 300°C under argon gas protection for 6 hours. After cooling to room temperature, the adsorption material is obtained, which is marked as Si@C-3.
[0028] Embodiment 4:
[0029] Weigh 10 kg of coal gangue powder (inorganic non-metallic mineral component content 88%, carbon content 12%), mix it thoroughly with 1 kg of sodium hydroxide, 0.2 kg of sodium silicate and 0.5 kg of ammonium persulfate, and then place it in a plasma ball mill, grind it for 40 minutes at a ball-to-material ratio of 2:1 and a rotation speed of 300 rpm, and then treat it with plasma discharge (frequency of 13.56 MHz) at a radio frequency power of 200 W for 100 seconds. The obtained product is calcined at a heating rate of 10°C / min and a temperature of 500°C under argon gas protection for 5 hours, and then cooled to room temperature to obtain an adsorption material, marked as Si@C-4.
[0030] Embodiment 5:
[0031] Weigh 10 kg of coal gangue powder (inorganic non-metallic mineral component content 90%, carbon content 10%), mix it thoroughly with 1.5 kg of sodium hydroxide and 0.6 kg of potassium persulfate, and then place it in a plasma ball mill, grind it for 40 minutes at a ball-to-material ratio of 1:1 and a rotation speed of 200 rpm, and then treat it with plasma discharge (frequency of 13.56 MHz) at a radio frequency power of 300 W for 120 seconds. The obtained product is calcined at a heating rate of 8 ° C / min and a temperature of 600 ° C under nitrogen gas protection for 3 hours. After cooling to room temperature, the adsorption material is obtained, which is marked as Si@C-5.
[0032] Structural characterization and performance of the product of the present invention: Through a series of technical characterizations, the microstructure morphology of the coal gangue powder and the product is observed. Figure 1 This is a scanning electron microscope photo of the raw material and the product. The raw material contains flake and block mineral components, while the microscopic morphology of the product is a uniform porous structure, indicating that the technology described above converts the various components of coal gangue into uniform amorphous silicates. Figure 2 The X-ray powder diffraction pattern shown also proves that the coal gangue is converted into amorphous silicate. Figure 3 The Raman spectra shown demonstrate the presence of carbon in the adsorbent material synthesized using coal gangue.
[0033] The BET specific surface area and pore structure parameters of the product are listed in Table 1, which proves that the product is a mesoporous material with a large specific surface area. The adsorption of lead ions, methylene blue and tetracycline in water by the raw materials and products is shown in Table 2. The maximum adsorption of lead ions, methylene blue and tetracycline by the prepared adsorbent material can reach 520.0 mg / g, 436.1 mg / g and 280.3 mg / g, respectively, which is 10 times, 13 times and 6 times the adsorption of coal gangue raw materials.
[0034] Table 1 Pore structure parameters of coal gangue powder and heterogeneous silicate adsorption materials
[0035]
[0036] Table 2 Adsorption capacity of coal gangue powder and heterogeneous silicate adsorption materials for Pb(II), methylene blue and tetracycline (initial concentration 400 mg / L)
[0037]
Claims
1. A method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling, characterized in that: The following steps are involved: The method comprises the following steps: crushing and sieving coal gangue to obtain coal gangue powder, taking a certain mass of coal gangue powder, alkali and oxidant and fully mixing them, then placing them in a plasma ball mill, grinding them for 10-60 minutes, and then treating them with plasma discharge for 20-300 seconds. The obtained product is calcined at a temperature range of 300-800°C for 1-6 hours under the protection of an inert gas, and then cooled to room temperature to obtain an adsorption material.
2. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The coal gangue is solid waste generated during coal mining or coal washing, wherein the content of inorganic non-metallic mineral components is 85% to 90% and the carbon content is 10% to 15%.
3. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The alkali is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate and potassium silicate.
4. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The amount of the alkali used is 10% to 100% of the mass of the coal gangue.
5. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The oxidant is one of hydrogen peroxide, potassium permanganate, ammonium persulfate and potassium persulfate, and the dosage is 5% to 20% of the mass of the coal gangue.
6. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The rotation speed of the ball mill is 100-1000 rpm, and the ball-to-material ratio is 1:1-3:
1.
7. The method for synthesizing heterogeneous silicate adsorption materials by reconstructing coal gangue using plasma ball milling according to claim 1, characterized in that: The radio frequency power of the plasma is 100-500W, the frequency is 13.56MHz, and the atmosphere is air.