Columnar activated carbon prepared from bamboo pyrolysis gasification waste and preparation method thereof
By preparing columnar activated carbon prepared by bamboo pyrolysis gasification waste, the problems of poor strength and difficulty in regeneration of bamboo activated carbon are solved, high value-added raw materials are provided, environmentally friendly production costs are reduced, and the application fields of activated carbon are broadened.
Patent Information
- Application Number
- CN202411027789.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The waste after pyrolyzed and gasified bamboo residue is directly prepared into powder or granular activated carbon, with poor strength, low loading density, difficulty in regeneration and recycling, and cannot meet the strength requirements of customers. The existing columnar activated carbon raw materials are limited, resulting in development Restricted.
The method of preparing columnar activated carbon by using bamboo pyrolysis gasification waste, including powder making, molding, low-temperature heat treatment, high-temperature heat treatment and post-treatment steps, using organic polymer compounds as binders, avoiding tar, and preparing through low-temperature and high-temperature heat treatment High added value columnar activated carbon.
Overcome the difficulties in regeneration of bamboo activated carbon, provide high value-added raw materials, reduce environmentally friendly production costs, improve the strength and application areas of activated carbon, broaden the utilization of bamboo resources, and reduce environmental and human pollution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of adsorption materials, and in particular to columnar activated carbon prepared from bamboo pyrolysis and gasification waste and a preparation method thereof. Background Art
[0002] my country is the world's most important bamboo producer and the country with the richest bamboo plants in the world. The bamboo industry has obvious development advantages and huge potential. Bamboo plants are important forest resources, with the characteristics of fast production, short production cycle, sustainable utilization after one-time cultivation, and wide range of uses. They have become important afforestation and beautification tree species for accelerating national greening and improving the ecological environment in my country. Therefore, a large amount of bamboo processing residues are generated every year. Usually, bamboo processing residues are used for pyrolysis and gasification for heating and power generation. The waste after pyrolysis and gasification is directly prepared into powdered activated carbon or granular activated carbon. However, the activated carbon prepared by this method has poor strength, low packing density, and is difficult to regenerate and recycle. It cannot meet customers' strength requirements for activated carbon, which limits the further application of bamboo activated carbon products.
[0003] Columnar activated carbon is a shaped activated carbon made by bonding and activating biomass powder or coal powder through a certain process. The preparation process is mature and stable. The shaped activated carbon produced has the advantages of good wear resistance, high filling density, and convenient regeneration and recycling. It is widely used in water purification, adsorption of harmful gases, catalyst carriers, etc., and has broad development prospects.
[0004] At present, the raw materials used to prepare molded activated carbon are mainly wood and coal. Due to the over-exploitation of wood resources and the non-renewable coal resources, the development of columnar activated carbon is limited by raw materials. In addition, in the preparation process of molded activated carbon, tar is needed as a binder, which not only causes pollution and harm to the environment and human body during the production process, but also requires tail gas treatment equipment, which requires a large investment. Summary of the invention
[0005] In order to solve the problems that the current output of bamboo processing residues is large and is usually used for pyrolysis and gasification, and the waste after pyrolysis and gasification is directly prepared into powdered activated carbon or granular activated carbon, the activated carbon has poor strength, low packing density, and is difficult to regenerate and recycle, while the columnar activated carbon with superior performance is limited by raw materials and development, the present invention provides a columnar activated carbon prepared from bamboo pyrolysis and gasification waste and a preparation method thereof.
[0006] The present invention is implemented by the following technologies: The present invention provides a method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, comprising the following steps: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%.
[0007] b. Molding The powder, binder and water are uniformly stirred and kneaded in a kneader to obtain a molding material. The binder is added in an amount of 10-50%, and the water is added in an amount of 20-40%. The binder is an organic polymer compound; the organic polymer compound includes a mixture of one or both of high viscosity powder and starch. Specifically, the organic polymer compound includes a mixture of 2 parts of high viscosity powder and 1 part of starch, so as to avoid damage to the environment and human body during storage, transportation and use when tar is used as a binder.
[0008] c. Low temperature heat treatment The formed material is placed in a converter for low temperature heat treatment at 100-600°C, the treatment temperature gradually increases with the extension of the treatment time, and the low temperature heat treatment time is 30-120 minutes. Further, the temperature of the low temperature heat treatment is 400-600°C, and the time is 30-50 minutes.
[0009] d. High temperature heat treatment The material after low temperature heat treatment is placed in a converter for high temperature heat treatment at 750-950°C, water vapor is passed during the high temperature heat treatment, the amount of water vapor is 0.1 ml / min•g, and the high temperature heat treatment time is 90-210 minutes. Furthermore, the temperature of the high temperature heat treatment is 800-900°C, and the time is 90-180 minutes.
[0010] e. Post-processing The activated material after high-temperature heat treatment is cooled and sieved, and the powder generated in the preparation process is removed to obtain bamboo columnar activated carbon.
[0011] The present invention also provides columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to the method.
[0012] Compared with the prior art, the present invention has the following beneficial effects: The method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste provided by the present invention uses bamboo as a raw material to prepare renewable and reusable columnar activated carbon, which overcomes the problem of difficulty in regenerating powdered activated carbon prepared from original bamboo pyrolysis and gasification waste. It can not only improve the high added value utilization of bamboo resources, but also provide abundant raw materials for the preparation of columnar activated carbon.
[0013] Moreover, the present invention does not need to add tar as a binder, which reduces the damage to the environment and human body caused by storage, transportation and use of tar as a binder, reduces environmentally friendly production costs, and has good research value and development prospects.
[0014] In addition, the present invention solves the problem of low strength of crushed granular activated carbon through process improvement. On the one hand, it ensures the cold strength of the formed sample, and on the other hand, it ensures the strength of the sample after subsequent high-temperature treatment, thereby broadening the application field of activated carbon. DETAILED DESCRIPTION
[0015] The specific embodiments of the present invention are described in detail below. Example 1
[0016] A method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, the specific steps are as follows: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%.
[0017] b. Molding In a kneader, powder, binder and water are mixed evenly and kneaded into a molding material. The binder is added in a ratio of 10% of the powder, and the water is added in a ratio of 20% of the powder. The binder is a mixture of high viscosity powder and starch in a ratio of 2:1.
[0018] c. Low temperature heat treatment The formed material is placed in a converter for low temperature heat treatment at 600°C. The treatment temperature is gradually increased with the extension of the treatment time. The low temperature heat treatment time is 30 minutes.
[0019] d. High temperature heat treatment The material after low-temperature heat treatment is placed in a converter for high-temperature heat treatment at 900°C. Steam is passed through the material during the high-temperature heat treatment. The amount of steam used is 0.1 ml / min•g. The high-temperature heat treatment time is 180 minutes.
[0020] e. Post-processing The activated material after high-temperature heat treatment is cooled and sieved, and the powder generated in the preparation process is removed to obtain bamboo columnar activated carbon. Example 2
[0021] A method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, the specific steps are as follows: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%.
[0022] b. Molding In a kneader, powder, binder and water are mixed evenly and kneaded into a molding material. The binder is added in a ratio of 15% of the powder, and the water is added in a ratio of 30% of the powder. The binder is a mixture of high-viscosity powder and starch in a ratio of 2:1.
[0023] c. Low temperature heat treatment The formed material is placed in a converter for low temperature heat treatment at 500°C. The treatment temperature increases gradually with the extension of the treatment time. The low temperature heat treatment time is 40 minutes.
[0024] d. High temperature heat treatment The material after low-temperature heat treatment is placed in a converter for high-temperature heat treatment at 850°C. Steam is passed through the material during the high-temperature heat treatment. The amount of steam used is 0.1 ml / min•g. The high-temperature heat treatment time is 90 minutes.
[0025] e. Post-processing The activated material after high-temperature heat treatment is cooled and sieved, and the powder generated in the preparation process is removed to obtain bamboo columnar activated carbon. Example 3
[0026] A method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, the specific steps are as follows: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%.
[0027] b. Molding In a kneader, powder, binder and water are mixed evenly and kneaded into a molding material. The binder is added in a ratio of 30% of the powder, and the water is added in a ratio of 40% of the powder. The binder is a mixture of high-viscosity powder and starch in a ratio of 2:1.
[0028] c. Low temperature heat treatment The formed material is placed in a converter for low temperature heat treatment at 400°C. The treatment temperature increases gradually with the extension of the treatment time. The low temperature heat treatment time is 50 minutes.
[0029] d. High temperature heat treatment The material after low-temperature heat treatment is placed in a converter for high-temperature heat treatment at 800°C. Steam is passed through the material during the high-temperature heat treatment. The amount of steam used is 0.1 ml / min•g. The high-temperature heat treatment time is 90 minutes.
[0030] e. Post-processing The activated material after high-temperature heat treatment is cooled and sieved, and the powder generated in the preparation process is removed to obtain bamboo columnar activated carbon. Example 4
[0031] A method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, the specific steps are as follows: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%.
[0032] b. Molding In a kneader, the powder, binder and water are mixed evenly and kneaded into a molding material. The binder is added in a ratio of 25% of the powder, and the water is added in a ratio of 40% of the powder. The binder is a mixture of high-viscosity powder and starch in a ratio of 2:1.
[0033] c. Low temperature heat treatment The formed material is placed in a converter for low temperature heat treatment at 500°C. The treatment temperature increases gradually with the extension of the treatment time. The low temperature heat treatment time is 30 minutes.
[0034] d. High temperature heat treatment The material after low-temperature heat treatment is placed in a converter for high-temperature heat treatment at 850°C. Steam is passed through the material during the high-temperature heat treatment. The amount of steam used is 0.1 ml / min•g. The high-temperature heat treatment time is 120 minutes.
[0035] e. Post-processing The activated material after high-temperature heat treatment is cooled and sieved, and the powder generated in the preparation process is removed to obtain bamboo columnar activated carbon.
[0036] Examples 1 to 4 and purchased commercial samples were taken to test the specific surface area, water capacity, iodine value, strength, and ash content. The results are shown in the following table:
[0037] The test results show that the test results of the samples in the embodiment are close to those of the purchased samples, but the raw material and processing costs are significantly lower. Bamboo can be used as a raw material to prepare renewable and reusable columnar activated carbon as an alternative product to purchased samples, saving production costs.
[0038] The present invention also provides columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to the method.
[0039] The scope of protection claimed by the present invention is not limited to the above specific embodiments. For those skilled in the art, the present invention may have various deformations and changes. Any modifications, improvements and equivalent substitutions made within the concept and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste, characterized in that: The following steps are involved: a. Flour milling The bamboo waste after pyrolysis and gasification is taken as raw material, and ground into powder with a fineness of 200 mesh and a passing rate of more than 95%; b. Molding The powder, binder and water are stirred evenly and kneaded to form a molding material, wherein the binder is added in an amount of 10-50% of the powder, the water is added in an amount of 20-40% of the powder, and the binder is an organic polymer compound; c. Low temperature heat treatment The formed molding material is placed in a low temperature heat treatment at 100-600°C for 30-120 minutes; d. High temperature heat treatment The material after low-temperature heat treatment is placed in a high-temperature heat treatment at 750-950°C, water vapor is passed during the high-temperature heat treatment, the water vapor dosage is 0.1 ml / min•g, and the high-temperature heat treatment time is 90-210 minutes; e. Post-processing The activated material after high temperature heat treatment is cooled and sieved to obtain bamboo columnar activated carbon.
2. The method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to claim 1, characterized in that: In step b, the organic polymer compound includes one or a mixture of high viscosity flour and starch.
3. The method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to claim 1, characterized in that: In step b, the stirring is carried out in a kneader.
4. The method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to claim 1, characterized in that: In step c, the temperature of the low-temperature heat treatment is 400-600° C., and the time is 30-50 minutes; in step d, the temperature of the high-temperature heat treatment is 800-900° C., and the time is 90-180 minutes.
5. The method for preparing columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to claim 1, characterized in that: In step d, high temperature heat treatment is performed in a converter.
6. A columnar activated carbon prepared from bamboo pyrolysis and gasification waste according to claim 1.
Citation Information
Patent Citations
Method for preparing activated carbon
CN111661846A
Method for producing columnar large-particle activated carbon by cold press molding of bamboo wastes
CN115072719A
Method for preparing composite activated carbon from multi-source carbonaceous raw materials
CN115722192A
Columnar activated carbon produced from bamboo waste
CN117361525A
Columnar activated carbon and preparation method thereof
CN117401677A