Lignin-based super-crosslinked resin as well as preparation method and application thereof
Through the preparation of lignin-based supercrosslinked resin, the efficiency and cost problems of aniline pollution treatment in water bodies are solved, and efficient adsorption and reuse are achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410963189.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to efficiently treat aniline contamination in water bodies, and traditional methods have problems of high cost and low efficiency, especially in reuse and industrial applications.
Using lignin as a raw material, combined with dimethoxymethane and a catalyst through Fuker alkylation reaction, a supercrosslinked resin with a large specific surface area and a porous structure was prepared for adsorption and removal of aniline in water.
It has achieved efficient adsorption of aniline, has good reusable performance and industrial application potential, has a large specific surface area of the resin, can maintain high efficiency in multiple uses, and is suitable for the treatment of water pollutants.
Smart Images

Figure CN118925681A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adsorption resins, and in particular to a lignin-based super-crosslinked resin and a preparation method and application thereof. Background Art
[0002] Aniline is a major additive for dyes, medicines, resins, rubber additives, etc., and is inevitably discharged into water bodies during industrial production. Due to its high toxicity and strong bioaccumulation ability, how to efficiently treat aniline in water bodies has become a hot topic of current research. The adsorption method is simple to operate, highly efficient, and can be reused. It is currently an ideal method for treating aniline wastewater. Due to its large specific surface area, unique pores, and rich functional groups, high cross-linked resins (HCPs) show great potential in the fields of removing organic pollutants, capturing gases, and removing heavy metals, and can be used to treat aniline in wastewater.
[0003] Highly cross-linked resins (HCPs) are a new type of polymer material first discovered by Davankov. In recent years, HCPs have been rapidly developed due to their diverse synthesis methods, large specific surface area, low raw material prices, safety and reliability. On this basis, other functional groups are further introduced to give the material specific properties. Initially, HCPs were made of linear polystyrene and a variety of cross-linking agents (divinylbenzene, p-xylene dichloride, chloromethyl methyl ether, etc.) were used to synthesize HCPs with a specific surface area of up to 1106 m 2 g -1 The reason why HCPs have such a large specific surface area is mainly due to the Friedel-Crafts alkylation of the crosslinking agent and the benzene ring. The covalent bridge formed after crosslinking turns the crosslinked network into a rigid structure, avoiding the collapse of the space between molecular chains caused by atomic stacking and forming permanent pores in the polymer chain.
[0004] Lignin is a potential renewable energy source, accounting for about 1 / 3 of the total amount of plants, and is an important component second only to cellulose. Lignin is a three-dimensional network macromolecule rich in aromatic rings and an important green environmentally friendly material. How to efficiently develop and utilize this environmentally friendly renewable resource is the focus of current scientific research. Summary of the invention
[0005] The purpose of the present invention is to provide a lignin-based super-crosslinked resin and a preparation method and application thereof. The preparation method is simple, the raw material source is wide, and it is easy to realize industrial application. The prepared lignin-based super-crosslinked resin has a large specific surface area and has good adsorption performance for organic matter such as aniline. It can be reused many times and has a high utilization rate.
[0006] The technical solution of the present invention is achieved in this way:
[0007] The invention provides a preparation method of a lignin-based super cross-linked resin, comprising the following steps: adding acidic lignin to 1,2-dichloroethane, stirring and swelling at room temperature, then adding dimethoxymethane and a catalyst, heating and stirring for pre-cross-linking, heating and continuing the reaction, washing with hydrochloric acid and anhydrous ethanol in sequence, then heating and refluxing Soxhlet extraction with alcohol, taking out the product, and drying to obtain the lignin-based super cross-linked resin.
[0008] As a further improvement of the present invention, the swelling time is 2-4 hours.
[0009] As a further improvement of the present invention, the catalyst is at least one of anhydrous ferric chloride, anhydrous bismuth trichloride, 1,3,5-triphenylbenzene, and 1,4-dichlorobenzyl.
[0010] As a further improvement of the present invention, the pre-crosslinking temperature is 40-50° C. and the time is 4-6 hours.
[0011] As a further improvement of the present invention, the temperature for continuing the reaction is 80-90° C. and the time is 45-50 hours.
[0012] As a further improvement of the present invention, the Soxhlet extraction time is 115-125 hours, and the alcohol is methanol or ethanol.
[0013] As a further improvement of the present invention, the product is further extracted by heating reflux with acetone for 22-26 hours.
[0014] As a further improvement of the present invention, the mass ratio of the acidic lignin, dimethoxymethane and catalyst is 10-10.2:23-31:6.4-60.
[0015] The present invention further protects a lignin-based super-crosslinked resin prepared by the above preparation method.
[0016] The present invention further protects the use of the above lignin-based super-crosslinked resin in the adsorption and removal of aniline.
[0017] The present invention has the following beneficial effects: the preparation method of the lignin-based super-crosslinked resin of the present invention is simple, the raw material source is wide, and it is easy to realize industrial application; the prepared lignin-based super-crosslinked resin has a large specific surface area, has good adsorption performance for organic matter such as aniline, can be reused many times, and has a high utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0019] Figure 1 is the infrared spectrum;
[0020] Figure 2 are scanning electron microscopy images; from top to bottom: HCPs-1 to HCPs-6);
[0021] Figure 3 is the standard curve of aniline solution;
[0022] Figure 4 is the adsorption isotherm of aniline on different resins at 25°C;
[0023] Figure 5 is the adsorption isotherm of HCPs-3 to aniline at different temperatures;
[0024] Figure 6 is the adsorption kinetic curve of aniline by HCPs-3;
[0025] Figure 7 This is the relationship curve between the amount of HCPs-3 and the adsorption efficiency of aniline;
[0026] Figure 8 The reusability of HCPs-3 resin;
[0027] Fig. 9 The effect of pH on the adsorption of aniline by HCPs-3 resin. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] Take 10.00g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (23.50g, 309.21mmol) and anhydrous ferric chloride (45.03g, 277.96mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it and form a polymer prototype, then heat it to 85℃ and continue the reaction for 48h until complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, then heated and refluxed with methanol for Soxhlet extraction for 48h, then heated and refluxed with acetone for extraction for 24h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain the hyper-crosslinked resin HCPs-1.
[0031] Example 2
[0032] Take 10.06g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (24.04g, 316.32mmol) and anhydrous bismuth trichloride (6.47g, 20.54mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it and form a polymer prototype, then heat it to 85℃ and continue the reaction for 48h until complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, then heated and refluxed with methanol for Soxhlet extraction for 48h, then heated and refluxed with acetone for extraction for 24h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain the hyper-crosslinked resin HCPs-2.
[0033] Example 3
[0034] Take 10.04g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (30.08g, 395.79mmol), 1,3,5-triphenylbenzene (3.42g, 11.18mmol), and anhydrous ferric chloride (55.12g, 340.25mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it to form a polymer prototype, and then heat it to 85℃ and continue the reaction for 48h until it is complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, and then heated and refluxed with ethanol for Soxhlet extraction for 120h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain the hyper-crosslinked resin HCPs-3.
[0035] Example 4
[0036] Take 10.07g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (30.08g, 395.79mmol), 1,3,5-triphenylbenzene (3.41g, 11.14mmol), and anhydrous bismuth trichloride (6.44g, 20.44mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it to form a polymer prototype, and then heat it to 85℃ and continue the reaction for 48h until complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, and then heated and refluxed with ethanol for Soxhlet extraction for 120h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain a super crosslinked resin HCPs-4.
[0037] Example 5
[0038] Take 10.14g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (29.99g, 394.61mmol), 1,4-dichlorobenzyl (1.99g, 11.37mmol), and anhydrous ferric chloride (54.77g, 338.09mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it to form a polymer prototype, and then heat it to 85℃ and continue the reaction for 48h until complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, and then heated and refluxed with ethanol for Soxhlet extraction for 120h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain the hyper-crosslinked resin HCPs-5.
[0039] Example 6
[0040] Take 10.13g of acidic lignin and 180mL of 1,2-dichloroethane and add them to the prepared 250mL dry round-bottom flask, and place it on a magnetic stirrer and stir and swell at room temperature for 3h. Then weigh dimethoxymethane (29.72g, 391.05mmol), 1,4-dichlorobenzyl (1.98g, 11.31mmol), and anhydrous bismuth trichloride (6.47g, 20.54mmol) and add them to the flask and stir evenly. Stir the reaction in a 45℃ oil bath for 5h to pre-crosslink it to form a polymer prototype, and then heat it to 85℃ and continue the reaction for 48h until complete. The obtained product is first washed with hydrochloric acid and anhydrous ethanol for 3 times, and then heated and refluxed with ethanol for Soxhlet extraction for 120h, take out the product, place the product in an oven at 80℃ and dry it for 2h, and finally dry it at 80℃ under reduced pressure for 6h to obtain the hyper-crosslinked resin HCPs-6.
[0041] Figure 1 is the infrared spectrum of each resin. Figure 1 In the infrared spectrum, 3650-3000cm -1 The vibration peak is generated by the stretching vibration of hydroxyl groups; at 3000-2800cm -1 The vibration peak at 1720cm is caused by the methylene stretching vibration; -1 The vibration peaks near the carbonyl group are generated by stretching vibration; at 1650-1400cm -1 The vibration peaks near the benzene ring are the vibration peaks of the benzene ring; -1 There is a vibration peak near the resin. The hydroxyl groups in the resin include both phenolic hydroxyl groups and alcoholic hydroxyl groups. At the same time, the vibration peak near this peak is also caused by the stretching vibration of the ether bond. It can be clearly seen from the figure that the two resins HCPs-1 and HCPs-2 have a peak at 3650-3000cm -1 The vibration peak intensity of HCPs-2 is significantly lower than that of other resins, indicating that its hydroxyl content should be lower than that of other resins; -1 There is no vibration peak nearby, indicating that it should not contain a carbonyl group.
[0042] The structure of the resin was characterized by scanning electron microscopy. Figure 2 From the above images, we can see that after the resin is magnified 5,000 times and 70,000 times, it is composed of many irregular small pieces connected together, with many pore structures, and the surface of the resin is smooth and rough. Among them, HCPs-3 has the most complex pore structure and the largest specific surface area.
[0043] Test Example 1 Adsorption Experiment
[0044] Test process:
[0045] (1) Drawing of standard curve of aniline solution
[0046] First prepare the solution: weigh 0.5g of aniline in a clean beaker, add a certain amount of deionized water and stir to dissolve, transfer to a 500mL volumetric flask, and dilute to the scale with deionized water. Shake evenly to obtain an aniline solution with a concentration of 1g / L. Then dilute the prepared 1g / L aniline solution to 15mg / L, 20mg / L, 25mg / L, 30mg / L, 35mg / L, 40mg / L, 45mg / L, 50mg / L, and 55mg / L in sequence. Finally, use a UV-visible spectrophotometer to test the absorbance of the diluted 9 concentrations of aniline solutions (the maximum absorption wavelength of aniline is 280nm) to obtain the absorbance of aniline solutions of each concentration. Then use origin to perform a linear fit between each concentration and its corresponding absorbance to obtain a standard curve of the aniline solution, as shown below: Figure 3 The standard curve formula for aniline is:
[0047] A=0.01421*C+0.00861(1)
[0048] Where A is the absorbance of aniline solution, C is the concentration of aniline solution, and their correlation coefficient R 2 Close to 1(R 2 =0.99978), indicating that the curve fitting effect is good.
[0049] (2) Thermodynamic experiment of resin adsorption on aniline
[0050] First, prepare 5 dry 100mL conical flasks, add 0.05g of dry HCPs-1 to each, and fully moisten with anhydrous ethanol and mark them, then add 50mL of aniline solution of five concentrations in turn (the five concentrations are: 101.66, 203.32, 304.98, 406.64, 508.3mg / L). Put the prepared conical flask in a water bath constant temperature oscillator, set the temperature to 25℃, and oscillate it at a constant temperature for 8 hours until the adsorption equilibrium is reached. After the oscillation is completed, take an appropriate amount of aniline aqueous solution, measure its absorbance, and calculate the equilibrium concentration of aniline after adsorption according to formula (1). At the same time, the equilibrium adsorption amount of aniline on the resin can be calculated using formula (2), and then the adsorption isotherm of HCPs-1 on aniline can be drawn. The equilibrium adsorption amount calculation formula is:
[0051] q e =(C0-C e )*V / m (2)
[0052] Among them, q e is the equilibrium adsorption amount, C0 is the initial concentration of aniline, C e is the equilibrium concentration, V is the volume of the solution, and m is the mass of the resin.
[0053] Similarly, the above method was used to conduct aniline adsorption experiments on HCPs-2, HCPs-3, HCPs-4, HCPs-5, and HCPs-6, and the adsorption isotherms of aniline on each resin were obtained. In particular, two different temperatures of 15°C and 35°C were added during the adsorption of HCPs-3 to conduct comparative experiments, and the adsorption isotherms of aniline on HCPs-3 at three temperatures were obtained.
[0054] (3) Adsorption kinetics of aniline by resin
[0055] Prepare a 250 mL conical flask, add 0.5 g of HCPs-3, fully moisten it with anhydrous ethanol, and add 250 mL of 400 mg / L aniline solution. Place the prepared conical flask in a water bath thermostatic oscillator, set the temperature to 15°C, oscillate at the constant temperature and start timing. Intermittently sample 1 mL of aniline solution at 0 min, 2 min, 4 min, 6 min, 8 min, 10 min, 15 min, 20 min, 25 min, 30 min, 40 min, 50 min, 60 min, 80 min, 100 min, 120 min, 150 min, 180 min, 210 min, 240 min, 270 min, 300 min, 330 min and 360 min, and measure its absorbance. Calculate the equilibrium concentration of aniline after adsorption according to formula (1). At the same time, use formula (2) to calculate the amount of aniline adsorbed by the resin at each moment. Then, use time t as the horizontal axis and the amount of aniline adsorbed by the resin at moment t as the vertical axis to draw the adsorption kinetic curve of the resin for aniline.
[0056] (4) Adsorption experiment of aniline by different resin dosages
[0057] Prepare 8 clean and dry conical flasks, add 0.0317g, 0.0499g, 0.1022g, 0.2037g, 0.3054g, 0.4093g, 0.5052g, 0.6064g of HCPs-3 respectively and mark them, add anhydrous ethanol to fully wet the resin, and then add 50mL of aniline solution with a concentration of 501.7mg / L. Put the prepared conical flask in a water bath constant temperature oscillator, set the temperature to 25℃, and oscillate it at a constant temperature for 8 hours until the adsorption equilibrium is reached. After the oscillation is completed, take a certain amount of aniline solution and measure its absorbance. Calculate the equilibrium concentration of aniline after adsorption according to formula (1), and calculate the adsorption efficiency of the resin for aniline (the adsorption efficiency is the initial concentration minus the equilibrium concentration divided by the initial concentration). Then, the equilibrium concentration of aniline is used as the horizontal coordinate, and the adsorption efficiency of the resin to aniline is used as the vertical coordinate to draw the adsorption curve of the resin to aniline under different resin concentration conditions.
[0058] (5) Resin reuse experiment
[0059] Take a clean and dry conical flask, add 0.1033g of HCPs-3, add anhydrous ethanol to fully wet the resin, and then add 50mL of aniline solution with a concentration of 500mg / L. Put the prepared conical flask in a water bath constant temperature oscillator, set the temperature to 25℃, and oscillate it at a constant temperature for 8 hours until adsorption equilibrium is reached. After the oscillation is completed, take an appropriate amount of aniline aqueous solution, measure its absorbance, and calculate its adsorption amount. Desorption method: filter out the resin, dry it, and then desorb it with 50ml of 60% ethanol and 0.1 mol / L hydrochloric acid for 5 hours. After desorption, filter out the resin, wash it alternately with ethanol and deionized water, place it in a vacuum dryer at 60℃, dry it, weigh it, and perform the adsorption-desorption test again. Repeat this 4 times for a total of 5 adsorption-desorption processes.
[0060] (6) Adsorption experiment of resin on aniline at different pH
[0061] Prepare an aniline solution with an original concentration of 405.84 mg / L, and adjust the pH of the solution with hydrochloric acid and sodium hydroxide. The pH values of the aniline solution are 2.914, 4.583, 5.482, 6.756, 8.911, and 11.094, respectively, and 50 mL each. Take a group of clean and dry conical flasks, add 0.05 g of HCPs-3, add anhydrous ethanol to fully wet the resin, and add the prepared aniline solution respectively. Then put the prepared conical flask in a water bath constant temperature oscillator, set the temperature to 25°C, and oscillate at a constant temperature for 8 hours until adsorption equilibrium. After the oscillation is completed, take a certain amount of aniline solution from it to measure its absorbance, calculate the equilibrium concentration of aniline after adsorption according to formula (1), and use formula (2) to calculate the amount of aniline adsorbed by the resin at each moment. The results are as follows.
[0062] (1) Adsorption isotherm
[0063] The obtained adsorption isotherm data were fitted with the Langmuir and Freundlich adsorption models, as shown in Figure 4 The adsorption isotherms of aniline for 6 kinds of resins at 25℃ show that the adsorption capacity of aniline for 6 kinds of resins is different. It can be seen from the Langmuir adsorption model data in Table 1 that the maximum adsorption capacity of the resins is 123.98412mg / g, 92.51503mg / g, 172.6456mg / g, 142.13657mg / g, 160.42812mg / g, and 87.28244mg / g. The largest one is 172.6456mg / g for HCPs-3, indicating that it has the best adsorption effect. Table 1 Freundlich adsorption model data K F(Freundlich constant, adsorption amount per unit concentration) The results are HCPs-3 (19.0752) > HCPs-5 (14.95904) > HCPs-1 (13.81279) > HCPs-6 (2.47378) > HCPs-2 (1.64131) > HCPs-4 (0.62386), which further shows that HCPs-3 has the strongest adsorption capacity for aniline.
[0064] Table 1 Adsorption equilibrium data of different resins fitted by Langmuir and Freundlich models
[0065]
[0066] On this basis, HCPs-3 was used to adsorb aniline at different temperatures (15°C, 25°C, and 35°C) to obtain the adsorption isotherms ( Figure 5 ) and Table 2. The results show that the two adsorption models can fit well. It is found that with the increase of temperature, the adsorption amount gradually increases, showing an endothermic reaction.
[0067] Table 2 Adsorption equilibrium data at different temperatures fitted by Langmuir and Freundlich models
[0068]
[0069]
[0070] (3) Adsorption kinetics
[0071] Figure 6 Table 3 shows the adsorption kinetics curve of aniline by resin HCPs-3 at three temperatures. Table 3 shows the pseudo-first-order and pseudo-second-order kinetic adsorption data. The initial concentration of aniline is 400 mg / L. The results show that the adsorption of aniline by the resin gradually increases with time, and its growth rate gradually decreases with time, and finally tends to equilibrium. The adsorption equilibrium can be reached in about 200 minutes. At the beginning of adsorption, there are many pore structures in the resin that do not adsorb aniline, which makes the adsorption of aniline increase rapidly. As time goes by, the pore structures that do not adsorb aniline gradually decrease, and the adsorption rate of aniline by the resin decreases accordingly, and finally tends to equilibrium.
[0072] Table 3 Pseudo-first-order and pseudo-second-order kinetic adsorption data
[0073]
[0074] (4) Effect of resin dosage on adsorption and reusability
[0075] Figure 7The relationship curve between the amount of HCPs-3 and the adsorption efficiency of aniline. In the solution, when the added resin increases from 0.0317g to 0.6064g, its adsorption efficiency increases rapidly from 18.2% to 96.6%. And as the resin concentration increases, the increase in adsorption efficiency slows down. When the added resin is greater than 0.5052g, the adsorption efficiency of the resin for aniline can reach more than 95%. After 5 adsorption-desorption cycles ( Figure 8 ), the adsorption amount is still 92.4% of the initial adsorption, showing good reusability.
[0076] (5) Effect of pH on aniline adsorption
[0077] Fig. 9 The relationship between the adsorption of aniline by the resin and the pH value is shown. The results show that the adsorption effect is better when the pH value is 4.583, indicating that the acidic state has the best adsorption effect. The results show that when the pH of the aniline solution is 4.583, its phenolic hydroxyl structure is relatively stable, and it is easy to form hydrogen bonds with amine molecules after adding aniline, and the adsorption performance is the best; but when the pH value drops from 4.583 to 2.914, due to the high acidity in the aniline solution, the resin and aniline are protonated, resulting in electrostatic repulsion, which is not conducive to the formation of hydrogen bonds. When pH>7, the added hydroxide can react with the phenolic hydroxyl, which is also not conducive to the formation of hydrogen bonds.
[0078] in conclusion:
[0079] In summary, this paper uses lignin as raw material, dimethoxymethane as crosslinking agent, two different catalysts and two different copolymers, and prepares 6 kinds of super crosslinked adsorption resins through Friedel-Crafts reaction. The prepared resin has a large specific surface area and many microporous structures. It is applied to the adsorption of aniline in aqueous solution. The adsorption experimental results show that HCPs-3 has the best adsorption effect on aniline at the same temperature; and at the three temperatures used in the experiment, the adsorption effect of the resin is the best at 35℃, and its maximum adsorption amount is 189.24597mg / g; the adsorption is best when the pH of the aniline solution is 4.583; it has good reusability; when the resin dosage is greater than 0.5052g, the adsorption efficiency of the resin on aniline can reach more than 95%.
[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a lignin-based super cross-linked resin, characterized in that: The method comprises the following steps: adding acidic lignin into 1,2-dichloroethane, stirring and swelling at room temperature, then adding dimethoxymethane and a catalyst, heating and stirring for pre-crosslinking, heating and continuing the reaction, washing with hydrochloric acid and anhydrous ethanol in sequence, then heating and refluxing with alcohol for Soxhlet extraction, taking out the product, drying, and obtaining a lignin-based super-crosslinked resin.
2. The preparation method according to claim 1, characterized in that: The swelling time is 2-4h.
3. The preparation method according to claim 1, characterized in that: The catalyst is at least one of anhydrous ferric chloride, anhydrous bismuth chloride, 1,3,5-triphenylbenzene and 1,4-p-dichlorobenzyl.
4. The preparation method according to claim 1, characterized in that: The pre-crosslinking temperature is 40-50° C. and the time is 4-6 hours.
5. The preparation method according to claim 1, characterized in that: The temperature for the continued reaction is 80-90°C and the time is 45-50h.
6. The preparation method according to claim 1, characterized in that: The Soxhlet extraction time is 115-125 hours, and the alcohol is methanol or ethanol.
7. The preparation method according to claim 1, characterized in that: The method further comprises heating the product with acetone under reflux for 22-26 hours.
8. The preparation method according to claim 1, characterized in that: The mass ratio of the acidic lignin, dimethoxymethane and catalyst is 10-10.2:23-31:6.4-60.
9. A lignin-based super-crosslinked resin obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the lignin-based super-crosslinked resin as claimed in claim 9 in the adsorption and removal of aniline.