Super-hydrophobic melamine sponge for dye degradation and emulsion purification and preparation method thereof
By combining Ag-MOF and hydroxyzinc fluoride nanoparticles with melamine sponges, a superhydrophobic sponge was prepared, which solved the problem of low adsorption capacity of existing sponges on organic dyes, achieved efficient oil-water separation and dye degradation, and was suitable for wastewater deal with.
Patent Information
- Application Number
- CN202411062299.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing superhydrophobic sponges have a low adsorption capacity and a slow adsorption rate, so they cannot effectively treat soluble dyes in wastewater, which limits their application range.
Ag-MOF and hydroxyzinc fluoride nanoparticles were synthesized by hydrothermal method, and combined with melamine sponge. Polydimethylsiloxane was used as a binder to prepare superhydrophobic and super lipophilic Ag-MOF@hydroxyl group Zinc fluoride @ polydimethylsiloxane @ melamine sponge to achieve efficient oil-water separation, dye degradation and emulsion purification.
The sponge has excellent performance in efficient oil-water separation and dye degradation, with a hydrophobic angle of 155.3°, an adsorption capacity of 54.6-109.7g/g, an oil-water separation efficiency of 99%, an emulsion purification efficiency of 98%, and a removal rate of malachite green can be achieved by Up to 99%, with extensive application prospects for wastewater treatment.
Smart Images

Figure CN118925683A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wastewater treatment composite materials, and particularly relates to a super-hydrophobic melamine sponge for dye degradation and emulsion purification and a preparation method thereof. Background Art
[0002] At present, water pollution is one of the major issues of global concern, which has caused huge economic losses and considerable harm to the ecosystem. Therefore, it is urgent to effectively remove oil substances, organic solvents and organic dyes from wastewater. Compared with other wastewater treatment technologies, adsorption is considered to be an efficient, low-cost and simple method. Among various adsorbent materials, sponges are widely used due to their porous structure, high adsorption capacity, reusability and easy recycling. In addition, sponges can be loaded with other nanoparticles by physical blending or chemical modification to greatly improve their adsorption performance.
[0003] Nano-metal organic frameworks (MOFs) have the characteristics of high porosity, high specific surface area, and high stability, so they occupy an important position in the field of adsorption. At present, many studies have successfully prepared MOF-based sponges for the removal of organic pollutants in wastewater, but most sponges have low adsorption capacity and slow adsorption rate for organic dyes. In addition, most superhydrophobic sponges can adsorb insoluble oil in oily wastewater, but cannot treat soluble dyes in wastewater, which limits their application. Therefore, it is of great significance to develop superhydrophobic sponges that can not only adsorb oil substances and organic solvents, but also efficiently degrade dyes. Summary of the invention
[0004] In order to solve the technical problems pointed out in the background technology part, the present invention provides a super hydrophobic melamine sponge for dye degradation and emulsion purification. With melamine as a substrate, Ag-MOF and hydroxyzinc fluoride nanoparticles are synthesized by a simple hydrothermal method, and the two nanoparticles are bonded to the melamine sponge using low surface energy material polydimethylsiloxane. Super hydrophobic and super oleophilic Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge is successfully prepared, which realizes efficient oil-water separation, dye degradation and emulsion purification, and can be widely used in the field of wastewater treatment.
[0005] The method for synthesizing Ag-MOF nanoparticles by hydrothermal method is as follows: 1.64g 2-methylimidazole is dissolved in 25mL ammonium hydroxide solution to obtain solution A; 0.58g silver nitrate is dissolved in 3mL deionized water to obtain solution B, solution B is slowly poured into solution A, stirred for 30min and then transferred to a high-pressure reactor, reacted at 100°C for 24h and then centrifuged, and the obtained solid is dried at 80°C for 12h to obtain Ag-MOF nanoparticles.
[0006] The hydrothermal method for synthesizing hydroxyzinc fluoride nanoparticles is as follows: 0.0891 g of alanine and 0.6585 g of zinc acetate dihydrate are dissolved in 25 ml of deionized water, and 0.1782 g of sodium hexafluorosilicate is added to the mixed solution after stirring for 30 minutes. After stirring for 30 minutes, the mixture is transferred to a high-pressure reactor, reacted at 120° C. for 12 hours, and then centrifuged. The obtained solid is dried at 70° C. for 4 hours to obtain hydroxyzinc fluoride nanoparticles.
[0007] The method for preparing superhydrophobic and superoleophilic Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge is as follows: a certain amount of Ag-MOF, hydroxyzinc fluoride and polydimethylsiloxane are added to 50 mL of n-hexane solution in a certain mass ratio, and after stirring for 30 min, 4 melamine sponges (volume: 1×1×1 cm) washed with ethanol and deionized water are added to the mixed solution. 3 ), stirred evenly and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0008] The mass ratio of Ag-MOF, hydroxyzinc fluoride and polydimethylsiloxane is 0.5:1:6-1:1:10, and the sponge stirring time is 1-4h.
[0009] The super-hydrophobic melamine sponge of the invention is used for dye degradation and emulsion purification.
[0010] The beneficial effects of the present invention are:
[0011] 1. The super-hydrophobic melamine sponge prepared by the present invention has the characteristics of simple preparation method, green and environmentally friendly preparation process, and readily available raw materials.
[0012] 2. Ag-MOF has uniform micropore size and high specific surface area (676m 2 / g), hydroxy zinc fluoride has the optimized geometric characteristics of nanotube assembled microspheres and a large specific surface area (271m 2 / g), and loading the two together on the melamine sponge is beneficial to promote the rapid adsorption of dyes.
[0013] 3. The super hydrophobic melamine sponge prepared by the present invention has excellent comprehensive performance. When the hydrophobic angle reaches 155.3°, its adsorption capacity still reaches 54.6-109.7 g / g. It also exhibits excellent oil-water separation ability (99%) and emulsion purification ability (98%). It also has efficient dye degradation ability under the condition of efficient oil-water separation, and the removal rate of malachite green can reach up to 99%. Therefore, the multifunctional modified sponge prepared by the present invention has broad application prospects in the field of wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the SEM image of the superhydrophobic melamine sponge obtained in Example 1.
[0015] Figure 2 1 is the XRD spectrum of Ag-MOF and hydroxyzinc fluoride in Example 1.
[0016] Figure 3 This is the SEM image of Ag-MOF and hydroxyzinc fluoride in Example 1.
[0017] Figure 4 This is a water contact angle diagram of the superhydrophobic melamine sponge obtained in Example 1.
[0018] Figure 5 The morphology of water drops on the original melamine sponge, the superhydrophobic melamine sponge obtained in Example 1 and its cross section.
[0019] Figure 6 Schematic diagram of the state of the original melamine sponge and the super hydrophobic and super oleophilic melamine sponge obtained in Example 1 in water.
[0020] Figure 7 This is a comparison chart of the adsorption capacity of the superhydrophobic melamine sponge obtained in Example 1 for different organic solvents or oil substances.
[0021] Figure 8 This is a comparison chart of the separation efficiency of the superhydrophobic melamine sponge obtained in Example 1 for different organic solvent / water mixtures.
[0022] Fig. 9 This is a comparison chart of the adsorption capacity of the superhydrophobic melamine sponge obtained in Example 1 after 10 cycles of adsorption of n-hexane and chloroform.
[0023] Fig.10 This is a comparison chart of the transmittance of the super hydrophobic melamine sponge obtained in Example 1 before and after purification of four emulsions of n-hexane in water, dichloromethane in water, n-hexane in water and dichloromethane in water.
[0024] Fig.11 This is a comparison chart of the removal rates of different dyes by the superhydrophobic melamine sponge obtained in Example 1.
[0025] Fig.12 This is a comparison chart of the removal rates of malachite green dye of different concentrations by the superhydrophobic melamine sponge obtained in Example 1.
[0026] Fig.13 This is a comparison chart of the removal rates of 10 mg / L malachite green within 1 hour by the original melamine sponge and the modified sponges obtained in Example 1, Comparative Example 1, and Comparative Example 2.
[0027] Fig.14The figure is a comparison chart of the hydrophobic angle and the adsorption capacity for n-hexane of the modified sponges obtained in Example 1, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with embodiments, but is not limited thereto.
[0029] Example 1
[0030] (1) 1.64 g of 2-methylimidazole was dissolved in 25 mL of ammonium hydroxide solution to obtain solution A; 0.58 g of silver nitrate solution was dissolved in 3 mL of deionized water to obtain solution B, solution B was slowly poured into solution A, stirred for 30 min, and then transferred to a high-pressure reactor, reacted at 100 ° C for 24 h, and then centrifuged. The obtained solid was dried at 80 ° C for 12 h to obtain Ag-MOF nanoparticles with a specific surface area of 676 m 2 / g.
[0031] (2) 0.0891 g of alanine and 0.6585 g of zinc acetate dihydrate were dissolved in 25 ml of deionized water, stirred for 30 min, 0.1782 g of sodium hexafluorosilicate was added to the mixed solution, stirred for 30 min, and then transferred to a high-pressure reactor. The mixture was reacted at 120 ° C for 12 h and then centrifuged. The obtained solid was dried at 70 ° C for 4 h to obtain hydroxy zinc fluoride nanoparticles with a specific surface area of 271 m 2 / g.
[0032] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0033] Figure 2 The XRD characterization results of Ag-MOF and hydroxyzinc fluoride are shown in Figure 2. In the XRD spectrum of Ag-MOF, prominent peaks are shown at 2θ of 16.9°, 28.0°, 28.8°, 39.4°, 44.3° and 65.4°, proving that Ag-MOF with high crystallinity has been successfully prepared. All diffraction peaks in the XRD spectrum of hydroxyzinc fluoride point to the orthorhombic phase of hydroxyzinc fluoride, and no other diffraction peaks caused by impurities are observed. Therefore, the prepared hydroxyzinc fluoride microspheres have high crystallinity and high purity.
[0034] Figure 3The SEM images of Ag-MOF and hydroxyzinc fluoride show that both Ag-MOF and hydroxyzinc fluoride are nanoparticles. Ag-MOF is formed by nanoparticle microclusters, while hydroxyzinc fluoride is a petal microsphere assembled from nanosheets. Both have rich pore structures, which are conducive to the adsorption of more dye molecules.
[0035] (i) The hydrophobic properties, saturated adsorption capacity, oil-water separation efficiency and reusability of the superhydrophobic melamine prepared by the present invention were further studied to evaluate the oil-water selectivity of the modified sponge.
[0036] (1) Hydrophobic properties
[0037] Figure 4 The hydrophobic angle diagram of Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge is as high as 155.3°. When deionized water is dropped on the surface of the original melamine sponge and the modified sponge, the water droplets on the original sponge are quickly absorbed, while the water droplets on the modified sponge remain spherical and the water droplets on its cross section also remain spherical ( Figure 5 ); When the original sponge and the modified sponge were placed in deionized water at the same time, the original sponge sank to the bottom of the water, while the modified sponge floated on the surface of the water ( Figure 6 ). Therefore, the super-hydrophobic melamine sponge prepared by the present invention has excellent super-hydrophobicity.
[0038] (2) Adsorption capacity for oil substances and organic solvents
[0039] like Figure 7 As shown, the adsorption capacity of Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge can reach 54.6 (n-hexane)-109.7 (chloroform) g / g, which has excellent adsorption capacity.
[0040] (3) Oil-water separation ability test
[0041] like Figure 8 As shown, the separation efficiency of the modified sponge for chloroform / water, n-hexane / water, dichloromethane / water, benzene / water, toluene / water and petroleum ether / water mixtures are 99.2%, 99.8%, 99.7%, 99.7%, 99.5% and 99.7%, respectively, and the oil-water separation efficiency all reaches 99%, which proves that the super hydrophobic melamine sponge prepared by the present invention has excellent oil-water separation performance.
[0042] (4) Reusability test
[0043] Reusability is of great significance in practical applications. The reusability of Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge was studied by cyclic adsorption-compression experiments. Fig. 9As shown, after 10 cycles, the adsorption capacity of the modified sponge for n-hexane and chloroform can still reach 51.6 g / g and 104.5 g / g, and the adsorption capacity only decreases by about 5%. Therefore, the super hydrophobic melamine sponge prepared by the present invention has excellent reusability.
[0044] (ii) Stable, miscible emulsions are more difficult to separate than incompatible oil-water mixtures. The modified sponge was experimentally investigated for its ability to purify water-in-chloroform, water-in-hexane, and water-in-toluene emulsions. The specific experimental steps are as follows:
[0045] Deionized water and n-hexane / dichloromethane were mixed at a volume ratio of 8:1 and stirred at high speed for 6 hours to prepare two water-in-oil emulsions (160 mL of deionized water and 20 mL of n-hexane / dichloromethane); deionized water and n-hexane / dichloromethane were mixed at a volume ratio of 1:8 and ultrasonicated for 30 minutes, and then 0.08 g of surfactant span80 (20 mL of deionized water and 160 mL of n-hexane / dichloromethane) was added and stirred for 6 hours to obtain two oil-in-water emulsions. The modified sponge was immersed in the four emulsions and the transmittance of the four emulsions before and after separation was measured using an ultraviolet spectrophotometer. Fig.10 As shown, the light transmittance of each emulsion after purification by the modified sponge is above 91%. Therefore, the modified sponge prepared by the present invention has high efficiency in emulsion purification.
[0046] (III) Most colored dyes are toxic and difficult to biodegrade due to their complex molecular structures. The removal rate of different dyes (all with a concentration of 10 mg / L) by the modified sponge within 150 minutes was investigated experimentally. Fig.11 As shown in the figure, the modified sponge has a strong adsorption effect on cationic dyes such as malachite green, and the removal rate of malachite green reaches 99.3%. The removal rate of malachite green of different concentrations by the modified sponge within 150 minutes was further investigated. Fig.12 As shown, within 150 minutes, the removal rates of the modified sponge for malachite green with concentrations of 5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L and 25 mg / L were 99.3%, 98.5%, 94.5%, 93.9% and 93.4% respectively, and the removal rates were all above 90%.
[0047] Example 2
[0048] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0049] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0050] (3) 0.05 g Ag-MOF, 0.025 g hydroxyzinc fluoride, and 0.3 g polydimethylsiloxane were added to 50 mL n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0051] The hydrophobic angle of the modified melamine sponge is 152.6°, the adsorption capacity for n-hexane is 52.8 g / g, and the separation efficiency of n-hexane / water mixture is 97.5%.
[0052] Example 3
[0053] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0054] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0055] (3) 0.025 g Ag-MOF, 0.05 g hydroxyzinc fluoride, and 0.3 g polydimethylsiloxane were added to 50 mL n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0056] The hydrophobic angle of the modified melamine sponge is 151.9°, the adsorption capacity for n-hexane is 52.4 g / g, and the separation efficiency of n-hexane / water mixture is 96.8%.
[0057] Example 4
[0058] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0059] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0060] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.1 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0061] The hydrophobic angle of the modified melamine sponge is 151.4°, the adsorption capacity for n-hexane is 53.4 g / g, and the separation efficiency of n-hexane / water mixture is 97.2%.
[0062] Example 5
[0063] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0064] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0065] (3) 0.05 g Ag-MOF, 0.05 g hydroxyzinc fluoride, and 0.2 g polydimethylsiloxane were added to 50 mL n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0066] The hydrophobic angle of the modified melamine sponge is 152.9°, the adsorption capacity for n-hexane is 54.1 g / g, and the separation efficiency of n-hexane / water mixture is 97.9%.
[0067] Example 6
[0068] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0069] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0070] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.4 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0071] The hydrophobic angle of the modified melamine sponge is 154.2°, the adsorption capacity for n-hexane is 53.2 g / g, and the separation efficiency of n-hexane / water mixture is 98.6%.
[0072] Example 7
[0073] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0074] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0075] (3) 0.05 g Ag-MOF, 0.05 g hydroxyzinc fluoride, and 0.5 g polydimethylsiloxane were added to 50 mL n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0076] The hydrophobic angle of the modified melamine sponge is 155.0°, the adsorption capacity for n-hexane is 52.9 g / g, and the separation efficiency of n-hexane / water mixture is 99.1%.
[0077] Example 8
[0078] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0079] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0080] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 1 hour and then cured at 180°C for 1 hour to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0081] The hydrophobic angle of the modified melamine sponge is 151.9°, the adsorption capacity for n-hexane is 50.2 g / g, and the separation efficiency of n-hexane / water mixture is 97.4%.
[0082] Example 9
[0083] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0084] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0085] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 2 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0086] The hydrophobic angle of the modified melamine sponge is 153.9°, the adsorption capacity for n-hexane is 53.8 g / g, and the separation efficiency of n-hexane / water mixture is 98.5%.
[0087] Example 10
[0088] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0089] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0090] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 4 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0091] The hydrophobic angle of the modified melamine sponge is 154.8°, the adsorption capacity for n-hexane is 52.4 g / g, and the separation efficiency of n-hexane / water mixture is 99.1%.
[0092] Comparative Example 1
[0093] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0094] (2) 0.1 g Ag-MOF and 0.3 g polydimethylsiloxane were added to 50 mL n-hexane solution and stirred for 30 min. Four melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@polydimethylsiloxane@melamine sponge.
[0095] The hydrophobic angle of the modified melamine sponge is 151.5°, the adsorption capacity for n-hexane is 46.9 g / g, the separation efficiency of n-hexane / water mixture is 97.4%, and the removal rate of malachite green with a concentration of 10 mg / L within 60 minutes is 96.5%.
[0096] Comparative Example 2
[0097] (1) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0098] (2) 0.1 g of hydroxy zinc fluoride and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain hydroxy zinc fluoride @ polydimethylsiloxane @ melamine sponge.
[0099] The hydrophobic angle of the modified melamine sponge is 152.0°, the adsorption capacity for n-hexane is 49.1 g / g, the separation efficiency of n-hexane / water mixture is 97.6%, and the removal rate of malachite green with a concentration of 10 mg / L within 60 minutes is 89.8%.
[0100] Comparative Example 3
[0101] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0102] (2) The preparation method of hydroxy zinc fluoride nanoparticles is the same as that in Example 1.
[0103] (3) 0.05 g Ag-MOF, 0.05 g hydroxyzinc fluoride, and 0.3 g polydimethylsiloxane were added to 50 mL n-hexane solution. After ultrasonication for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), and then cured at 180 °C for 1 h after ultrasonic treatment for 3 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0104] The hydrophobic angle of the modified melamine sponge is 153.2°, the adsorption capacity for n-hexane is 49.6 g / g, the separation efficiency of n-hexane / water mixture is 98.2%, and the removal rate of malachite green with a concentration of 10 mg / L within 60 minutes is 93.4%.
[0105] Comparative Example 4
[0106] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0107] (2) 0.2195 g of zinc acetate dihydrate was dissolved in 25 mL of ethylene glycol, and 0.3299 g of sodium tungstate dihydrate was added thereto after stirring for 30 min. The mixed solution was stirred for 30 min and then transferred to a high-pressure reactor. After reacting at 150° C. for 12 h, the mixture was centrifuged and the obtained solid was dried at 70° C. for 4 h to obtain zinc tungstate nanoparticles.
[0108] (3) 0.05 g Ag-MOF, 0.05 g zinc tungstate, and 0.3 g polydimethylsiloxane were added to 50 mL n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@zinc tungstate@polydimethylsiloxane@melamine sponge.
[0109] The hydrophobic angle of the modified melamine sponge is 151.8°, the adsorption capacity for n-hexane is 50.2 g / g, the separation efficiency of n-hexane / water mixture is 97.5%, and the removal rate of malachite green with a concentration of 10 mg / L within 60 minutes is 78.5%.
[0110] Comparative Example 5
[0111] (1) The preparation method of Ag-MOF nanoparticles is the same as that in Example 1.
[0112] (2) 0.0891 g of alanine and 0.6585 g of zinc acetate dihydrate were dissolved in 25 ml of deionized water. After stirring for 30 min, 0.1782 g of sodium hexafluorosilicate was added to the mixed solution. After stirring for 30 min, the mixture was transferred to a high-pressure reactor, reacted at 120° C. for 6 h, and then centrifuged. The obtained solid was dried at 70° C. for 4 h to obtain hydroxyzinc fluoride nanoparticles.
[0113] (3) 0.05 g of Ag-MOF, 0.05 g of hydroxyzinc fluoride, and 0.3 g of polydimethylsiloxane were added to 50 mL of n-hexane solution. After stirring for 30 min, 4 melamine sponges (volume: 1 × 1 × 1 cm) washed with ethanol and deionized water were added to the mixed solution. 3 ), stirred for 3 h and then cured at 180 °C for 1 h to obtain Ag-MOF@hydroxyzinc fluoride@polydimethylsiloxane@melamine sponge.
[0114] The hydrophobic angle of the modified melamine sponge is 153.8°, the adsorption capacity for n-hexane is 48.8 g / g, the separation efficiency of n-hexane / water mixture is 98.6%, and the removal rate of malachite green with a concentration of 10 mg / L within 60 minutes is 90.6%.
[0115] The above-described embodiments are only preferred examples for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A super hydrophobic melamine sponge, characterized in that: The super-hydrophobic melamine sponge is based on melamine, and Ag-MOF nanoparticles and hydroxy zinc fluoride nanoparticles are loaded on the melamine sponge by using polydimethylsiloxane to obtain a super-hydrophobic Ag-MOF@hydroxy zinc fluoride@polydimethylsiloxane@melamine sponge.
2. The super hydrophobic melamine sponge according to claim 1, characterized in that The preparation method of the Ag-MOF nanoparticles is as follows: dissolving 2-methylimidazole in an ammonium hydroxide solution to obtain a solution A; dissolving silver nitrate in deionized water to obtain a solution B; adding the solution B to the solution A, stirring for 30 minutes, and then transferring to a high-pressure reactor; and centrifugally drying after the reaction is complete to obtain the Ag-MOF nanoparticles.
3. The super hydrophobic melamine sponge according to claim 2, characterized in that The amount of 2-methylimidazole used was 1.64 g, the amount of ammonium hydroxide used was 25 mL, the amount of silver nitrate used was 0.58 g, and the amount of deionized water used was 3 mL; the reaction in the high-pressure reactor was maintained at 100° C. for 24 hours, and the drying was continued at 80° C. for 12 hours.
4. The super hydrophobic melamine sponge according to claim 1, characterized in that The preparation method of the hydroxy zinc fluoride nanoparticles is as follows: alanine and zinc acetate dihydrate are dissolved in deionized water, sodium hexafluorosilicate is added after stirring for 30 minutes, and after stirring until completely dissolved, the mixture is transferred to a high-pressure reactor, and after the reaction is complete, the mixture is centrifuged and dried to obtain the hydroxy zinc fluoride nanoparticles.
5. The super hydrophobic melamine sponge according to claim 4, characterized in that The amount of alanine used was 0.0891 g, the amount of zinc acetate dihydrate used was 0.6586 g, the amount of deionized water used was 25 mL, and the amount of sodium hexafluorosilicate used was 0.1782 g; the reaction in the high-pressure reactor was continued at 120° C. for 12 h, and the drying was maintained at 70° C. for 4 h.
6. The super hydrophobic melamine sponge according to claim 1, characterized in that: The mass ratio of Ag-MOF, hydroxyzinc fluoride and polydimethylsiloxane is 0.5:1:6-1:1:
10.
7. A method for preparing a super hydrophobic melamine sponge as claimed in claim 1, characterized in that: The preparation method comprises the following steps: adding Ag-MOF, hydroxy zinc fluoride and polydimethylsiloxane into a n-hexane solution according to a mass ratio, stirring for 30 minutes, adding a pretreated melamine sponge into the mixed solution, stirring evenly and then curing to obtain Ag-MOF@hydroxy zinc fluoride@polydimethylsiloxane@melamine sponge.
8. The method for preparing a super hydrophobic melamine sponge as claimed in claim 7, wherein: The pretreated melamine sponge was obtained by ultrasonicating in ethanol and deionized water for 1 h and then drying at 60 °C. The single volume was 1*1*1cm 3 , the input quantity is 4.
9. The method for preparing a super hydrophobic melamine sponge according to claim 7, wherein: The time for adding the sponge and stirring evenly is 1-4 hours, and the curing is maintained at 180°C for 1 hour.
10. A use of the super hydrophobic melamine sponge as claimed in claim 1, characterized in that: The super-hydrophobic melamine sponge is used for dye degradation and emulsion purification.
Citation Information
Patent Citations
Controllable synthesizing method for hydroxy zinc fluoride nanometer materials with different morphologies and environmental photocatalytic application of hydroxy zinc fluoride nanometer materials
CN109970098A
Preparation method and application of light-driven Janus super-hydrophobic sponge motor
CN115160732A