Oxygen vacancy-rich oxide loaded noble metal ruthenium dioxide catalyst as well as preparation method and application thereof
Through the preparation of the oxygen-enriched vacancies supported noble metal ruthenium dioxide catalyst, the stability and cost problems of the anode catalyst are solved, the electrochemical activity is improved and the cost is reduced, and the commercialization process of proton exchange membrane water electrolytic cell is promoted.
Patent Information
- Application Number
- CN202411089861.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The stability and cost issues of the anode catalyst in the existing proton exchange membrane water electrolytic cell (PEMWE) limit their large-scale applications, especially the poor stability of the ruthenium-based catalyst, which limits its industrial applications.
The preparation method of oxygen-rich vacancies supported by the noble metal ruthenium dioxide catalyst is used to prepare a highly active and cost-effective catalyst by stirring, heating and calcining the ruthenium source and the oxygen-rich vacancies support in water, thereby reducing the loading of precious metals. and improve electrochemical activity.
It has realized a catalyst that is corrosion-resistant and oxidative-decomposition, improved electrochemical activity, reduced costs, promoted the commercialization of proton exchange membrane water electrolytic cells, and provided a new solution for the industrial application of electrolytic water.
Smart Images

Figure CN118925716A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of electrocatalytic materials, and in particular to an oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst, and a preparation method and application thereof. Background Art
[0002] At present, the global energy structure and environmental pollution are becoming increasingly tense. In order to solve energy problems and environmental pollution, it is necessary to establish a clean and renewable energy cycle. Hydrogen energy has attracted the attention and support of governments of many countries in the world because of its high energy density and environmental protection and pollution-free.
[0003] Most of the hydrogen atoms on Earth exist in water by binding to oxygen, so the electrolysis of water using renewable electricity is widely regarded as a promising and sustainable way to produce clean hydrogen fuel. Proton exchange membrane water electrolyzer (PEMWE) is considered to be one of the most promising green hydrogen production technologies due to its advantages such as high operating current density, high energy efficiency, high hydrogen purity, compact system integration structure, and wide power fluctuation range. However, the life and cost of anode catalysts are the main bottlenecks restricting the large-scale application of proton exchange membrane water electrolyzer (PEMWE). Therefore, research on anode catalysts for proton exchange membrane (PEMWE) water electrolyzers is crucial. Due to the harsh chemical environment, only limited materials can be used as OER catalysts in acidic media. At present, iridium-based and ruthenium-based precious metal oxides are mainly used. Among them, the high cost of iridium-based precious metal catalysts limits its industrial-scale application. In contrast, ruthenium-based catalysts have high activity and low cost, but poor stability. Therefore, one problem that ruthenium-based catalysts need to overcome is their operational stability. Therefore, it is of great significance to develop durable and cost-effective Ru-based acidic OER catalysts for commercial application in PEM electrolyzers. Summary of the invention
[0004] In view of this, the embodiments of the present application provide an oxygen-rich vacancy oxide-loaded precious metal ruthenium dioxide catalyst and a preparation method and application thereof. The preparation method reduces the loading of the precious metal catalyst and improves the activity of the catalyst, reduces the cost of the acidic OER catalyst, is of great significance to promoting the commercialization process of proton exchange membrane water electrolyzer (PEMWE), and can effectively overcome the defects of the above-mentioned prior art.
[0005] The first aspect of the embodiment of the present application provides a method for preparing an oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst, comprising the following steps:
[0006] S1, dissolving a ruthenium source and an oxygen-rich vacancy oxide carrier in water, stirring evenly at room temperature to obtain a mixed solution;
[0007] S2, heating and stirring the mixed solution to obtain a black suspension, and filtering, washing, and drying the black suspension to obtain a precursor solid;
[0008] S3, calcining the precursor solid to obtain an oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst.
[0009] Specifically, the preparation method of the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst comprises the following steps:
[0010] A ruthenium source is dissolved in water to prepare solution A; an oxygen-rich vacancy oxide carrier is dissolved in water and dispersed evenly by ultrasonication to obtain solution B; solution A is added dropwise to solution B, stirred and mixed evenly to obtain solution C; solution C is stirred at high temperature to obtain a black suspension D; the black suspension D is filtered, washed, and dried to obtain a precursor solid; the precursor solid is calcined to obtain an oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst.
[0011] In some embodiments that may include the above embodiments, in step S1, the ruthenium source is RuCl3.XH2O, and the usage ratio of RuCl3.XH2O to oxygen-rich vacancy oxide is (1-20 mg):20 mg; or
[0012] In step S1, the stirring time at room temperature is 10-15h; or
[0013] In step S2, the heating and stirring temperature is 80-120° C., and the heating and stirring time is 12 h; or
[0014] In step S3, the specific calcination conditions are: placing in a muffle furnace under air atmosphere at a temperature of 100-400° C. at a heating rate of 2° C. / min for 2-6 hours.
[0015] In some embodiments that may include the above embodiments, in step S2, the specific washing conditions are: washing by suction filtration, the number of washing times is 3-5 times, the detergent is ultrapure water, and 15-50 ml is used each time; or
[0016] In step S2, the specific drying conditions are: placing in a blast drying oven and drying overnight, the temperature of the drying oven is 60-120°C, the drying time is 8-12h, or the drying is vacuum drying.
[0017] In some embodiments that may include the above embodiments, when the oxygen-rich vacancy oxide is oxygen-rich vacancy SnO2, the preparation process of the oxygen-rich vacancy SnO2 is:
[0018] Tin chloride pentahydrate, ethanol, ultrapure water and sodium hydroxide are mixed, stirred and ultrasonically treated to obtain a white mixed suspension; the white mixed suspension is then subjected to a sealed solvent thermal reaction at a temperature of 180-220°C for 24 hours. After the reaction is completed, the SnO2 light blue solid powder is obtained by centrifugation and ultrapure water washing; the SnO2 light blue solid powder is then dried at a temperature of 60-120°C for 8-12 hours to obtain a light blue SnO2 mineral crystal powder; the light blue SnO2 mineral crystal powder is kept at 350-550°C for 2-5 hours in a mixed atmosphere of argon and hydrogen to produce oxygen vacancies, and oxygen vacancy-rich SnO2 mineral crystal powder is obtained, which is marked as D-SnO2 mineral crystal powder.
[0019] Specifically, when the oxygen-rich vacancy oxide is oxygen-rich vacancy SnO2, the preparation process of the oxygen-rich vacancy SnO2 is:
[0020] Tin chloride pentahydrate, ethanol, ultrapure water and sodium hydroxide are mixed, stirred and ultrasonically treated to obtain a white mixed suspension; the white mixed suspension is then introduced into a 100 mL polytetrafluoroethylene liner and subjected to a sealed solvent thermal reaction at 180-220°C for 24 hours. After the reaction is completed, the SnO2 light blue solid powder is obtained by centrifugation and ultrapure water washing; the SnO2 light blue solid powder is then placed in a blast drying oven and dried overnight at 60-120°C for 8-12 hours to obtain a light blue SnO2 mineral crystal powder; the light blue SnO2 mineral crystal powder is placed in a tubular furnace and kept warm at 350-550°C for 2-5 hours in a mixed atmosphere of argon and hydrogen to produce oxygen vacancies, thereby obtaining oxygen vacancy-rich SnO2 mineral crystal powder, which is marked as D-SnO2 mineral crystal powder.
[0021] In some embodiments that may include the above embodiments, the usage ratio of tin chloride pentahydrate, ethanol, ultrapure water, and sodium hydroxide is 1.33g:(25ml-30ml):(25ml-30ml):1.26g, wherein the volume ratio of ultrapure water to ethanol is 1:1; or
[0022] The specific process of the stirring and ultrasonic treatment is: ultrasonic treatment for 0.5 h and stirring for 1 h are performed alternately 3-5 times.
[0023] In some embodiments that may include the above embodiments, the specific conditions of the centrifugation and ultrapure water washing are: washing after the reaction is completed and centrifuging with ultrapure water, washing 4-6 times with 20-30 ml of ultrapure water each time, the washing speed is 1200 r / min, and the washing time for each time is 10 min; or
[0024] The flow ratio of argon gas to hydrogen gas is 95:5, the flow rate of argon gas is 95 cc, and the flow rate of hydrogen gas is 5 cc.
[0025] In some embodiments that may include the above embodiments, when the oxygen-rich vacancy oxide is oxygen-rich vacancy TiO2, the preparation process of the oxygen-rich vacancy TiO2 is:
[0026] Titanyl sulfate, ethanol, ether and propylene glycol are mixed, stirred and ultrasonically treated to obtain a milky white mixed suspension; the milky white mixed suspension is then subjected to a sealed solvent thermal reaction at a temperature of 100-150°C for 12 hours, and after the reaction is completed, white solid TiO2 is obtained by vacuum filtration and alcohol washing; it is then dried overnight at a temperature of 60-80°C to obtain a white TiO2 hollow tube powder; the white TiO2 hollow tube powder is calcined at 550°C in an argon atmosphere for 2-5 hours to obtain a black TiO2 hollow tube powder; the black TiO2 hollow tube powder is etched in plasma for 1-3 minutes to produce oxygen vacancies, and the etching power is 300-600W to obtain oxygen vacancy-rich TiO2 powder, which is recorded as D-TiO2 hollow nanotube powder.
[0027] Specifically, when the oxygen-rich vacancy oxide is oxygen-rich vacancy TiO2, the preparation process of the oxygen-rich vacancy TiO2 is:
[0028] Titanyl sulfate, ethanol, ether and propylene glycol are mixed, stirred and ultrasonically treated to obtain a milky white mixed suspension; the milky white mixed suspension is then introduced into a 100 mL polytetrafluoroethylene liner for a sealed solvent thermal reaction at 100-150°C for 12 hours, and after the reaction is completed, a white TiO2 solid is obtained by vacuum filtration and alcohol washing; the solid is then placed in a blast drying oven and dried overnight at 60-80°C for 8-12 hours to obtain a white TiO2 hollow tube powder; the white TiO2 hollow tube powder is placed in a tubular furnace and calcined at 550°C for 3-5 hours under an argon atmosphere to obtain a black TiO2 hollow tube powder; the black TiO2 hollow tube powder is etched in plasma for 1-3 minutes to produce oxygen vacancies, and the etching power is 300-600W to obtain an oxygen vacancy-rich TiO2 powder, which is recorded as D-TiO2 hollow nanotube powder.
[0029] In some embodiments that may include the above embodiments, the titanyl sulfate, ethanol, ether and glycerol are used in a ratio of 1g:(25ml-30ml):(15ml-18ml):(15ml-18ml); or
[0030] The stirring and ultrasonic treatment specifically includes: stirring for 2 hours and ultrasonic treatment for 1 hour, alternately for 3-5 times; or
[0031] The vacuum filtration and alcohol washing specifically include: washing the white solid obtained by the thermal reaction of the sealed solvent, filtering with ethanol, and washing 4-6 times with 20-50 ml of ethanol each time.
[0032] The second aspect of the embodiment of the present application also provides an oxygen-rich vacancy oxide-loaded precious metal ruthenium dioxide catalyst, which is prepared by the above-mentioned method.
[0033] A third aspect of the embodiments of the present application also provides the use of the above-mentioned oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst in electrolysis of water.
[0034] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0035] (1) The oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst in the embodiments of the present application, on the one hand, processes the corrosion-resistant and oxidative decomposition-resistant semiconductor material into a carrier with good conductivity by creating oxygen vacancies, and on the other hand, improves the electrochemical activity and reduces the loading of the noble metal;
[0036] (2) The preparation method in the embodiment of the present application can be simply extended to the preparation of other oxygen-rich vacancy oxide-supported ruthenium dioxide catalysts. It is a universal method with universal applicability and can also be simply extended to other precious metals loaded onto oxygen-rich vacancy oxide carriers;
[0037] (3) The oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst in the examples of the present application exhibits relatively excellent electrochemical performance in electrolyzed water, providing a new research scheme for the industrial application of electrolyzed water; the hollow titanium-based nanotube-loaded noble metal ruthenium dioxide catalyst obtained by this preparation method has good application prospects in the fields of electrocatalysis, organic catalysis, and biodiagnosis and treatment, especially in promoting the industrialization process of catalysts with oxygen-rich vacancy oxides as carriers in electrolyzed water. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0039] Figure 1 Schematic diagram of the process for preparing RuO2 / D-SnO2 in Example 1 of the present application;
[0040] Figure 2 Schematic diagram of the process for preparing RuO2 / D-TiO2 in Example 2 of the present application;
[0041] Figure 3 is the XRD pattern of D-SnO2 in Example 1 of the present application;
[0042] Figure 4 is the XRD pattern of RuO2NPs / D-SnO2 in Example 1 of the present application;
[0043] Figure 5 This is the XRD pattern of D-TiO2 in Example 2 of the present application;
[0044] Figure 6 is the XRD pattern of RuO2NPs / D-TiO2 in Example 2 of the present application;
[0045] Figure 7 This is the EPR diagram of D-SnO2 in Example 1 of the present application;
[0046] Figure 8 This is the EPR diagram of D-TiO2 in Example 2 of the present application;
[0047] Fig. 9 This is the SEM image of D-SnO2 in Example 1 of the present application;
[0048] Fig.10 This is the SEM image of RuO2 / D-SnO2 in Example 1 of the present application;
[0049] Fig.11 This is the SEM image of D-TiO2 in Example 2 of the present application;
[0050] Fig.12 This is the SEM image of RuO2 / D-TiO2 in Example 2 of the present application;
[0051] Fig.13 TEM image of RuO2 / D-SnO2 in Example 1 of the present application;
[0052] Fig.14 The OER polarization curve of the RuO2 / D-SnO2 catalyst in 0.5M H2SO4 in Example 1 of the present application;
[0053] Fig.15 The OER polarization curve of the RuO2 / D-TiO2 catalyst in 0.5M H2SO4 in Example 2 of the present application;
[0054] Fig.16 The OER polarization curve of the RuO2 / D-SnO2 catalyst in 0.5M H2SO4 in Example 1 of the present application;
[0055] Fig.17 This is the OER polarization curve of the RuO2 / D-TiO2 catalyst in 0.5M H2SO4 in Example 2 of the present application. DETAILED DESCRIPTION
[0056] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0057] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.
[0058] In the following examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0059] Currently in the field of electrochemical water splitting, the development of high-performance acidic OER electrocatalysts with excellent activity and durability is a key issue in promoting the large-scale application of PEM electrolyzers in large-scale hydrogen production.
[0060] High-performance electrocatalysts should have the following advantages: good catalytic activity and acceptable cost. Due to the harsh chemical environment, only limited materials can catalyze OER in acidic media, and oxides of iridium-based and ruthenium-based noble metals are currently mainly used. The high price of precious metal iridium limits its commercial application. Precious metal Ru is the cheapest platinum group metal (Ru: $845 / ounce, platinum: $1226 / ounce, palladium: $2918 / ounce and Ir: $6750 / ounce). Volcano theory. Ruthenium dioxide is located near the top of the volcano among the widely studied oxides, indicating the excellent potential of ruthenium dioxide as an ideal candidate for OER. In terms of electrochemical activity, there is still a lot of room for improvement due to the space between ruthenium dioxide and the top of the volcano. Therefore, it has great development prospects to improve its catalytic activity in acidic OER and reduce its cost based on ruthenium dioxide.
[0061] Example 1
[0062] like Figure 1 As shown, the preparation method of the oxygen-rich vacancy SnO2-loaded noble metal ruthenium dioxide catalyst in this embodiment specifically includes the following steps:
[0063] S1. Preparation of D-SnO2 mineral crystal carrier:
[0064] 1.33 g of tin chloride pentahydrate, 25 ml of ethanol, 25 ml of ultrapure water and 1.26 g of sodium hydroxide were placed in a 100 ml beaker and stirred and ultrasonically treated (ultrasonication for 0.5 h and stirring for 1 h were performed alternately for 3-5 times) to obtain a white mixed suspension; the white mixed suspension was then introduced into a 100 mL polytetrafluoroethylene liner for a sealed solvent thermal reaction for 24 h, and the sealed solvent thermal reaction temperature was 200 ° C; after the reaction was completed, the mixture was centrifuged and washed with ultrapure water (washed and centrifuged with ultrapure water, 25 ml of ultrapure water was used for washing 6 times each time, the washing speed was 1200 r / min, and the washing speed was 1200 r / min. time is 10min) to obtain SnO2 light blue solid powder; then put it into a blast drying oven and dry it overnight, and the temperature of the blast drying oven is 60℃, and the drying time is 8-12h to obtain light blue SnO2 mineral crystal powder; finally, 5g of light blue SnO2 mineral crystal powder is placed in a tubular furnace, and high-purity argon gas is first introduced to replace the air in the furnace tube, and then it is kept warm for 2h at 450℃ in an argon and hydrogen mixed atmosphere (the flow ratio of argon and hydrogen is 95cc:5cc, the argon flow rate is 95cc, and the hydrogen flow rate is 5cc) to obtain oxygen vacancy-rich SnO2 mineral crystal powder, which is called D-SnO2 mineral crystal powder.
[0065] Preparation of S2, RuO2 / D-SnO2 catalysts:
[0066] Weigh 20 mg of D-SnO2 carrier and 2 ml (10 mg / ml) of RuCl3.XH2O, disperse them in an aqueous solution and place them in a 100 ml beaker. After uniform stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 110°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on D-SnO2. Collect the solid product by filtration, wash it three times with ultrapure water, each time with 15 ml of ultrapure water, and dry it in vacuum; finally, keep it in a muffle furnace at 300°C for 2 hours with a heating rate of 2°C / min.
[0067] Figure 3 Through X-ray diffraction phase analysis (XRD), it was found that D-SnO2 and the standard card PDF-77-0449 of tin dioxide matched well, proving that the carrier was successfully prepared. Figure 4 Through X-ray diffraction phase analysis (XRD), it was found that RuO2NPs / D-SnO2 matched well with the standard card PDF-77-0449 of tin dioxide and the standard card PDF-43-1027 of rutile ruthenium dioxide, proving that the catalyst was successfully prepared. Figure 7 Electron paramagnetic resonance (EPR) was used to demonstrate the successful preparation of tin dioxide oxygen vacancies.
[0068] Fig. 9 Scanning electron microscopy (SEM) was used to observe that D-SnO2 was in the form of mineral crystals. Fig.10The morphology of oxygen vacancy-rich crystalline tin dioxide supported noble metal ruthenium dioxide catalyst was observed by scanning electron microscopy (SEM). Fig.13 It can be seen from a transmission electron microscope (TEM) that the ruthenium dioxide prepared in this example is uniformly dispersed on the oxygen-rich tin dioxide carrier.
[0069] Example 2
[0070] like Figure 2 As shown, the preparation method of the oxygen vacancy-rich TiO2-loaded noble metal ruthenium dioxide catalyst in this embodiment specifically includes the following steps:
[0071] S1. Preparation of D-TiO2 hollow nanotube carrier:
[0072] In a fume hood, add 28 ml of ethanol, 16 ml of ether and 16 ml of propylene glycol to a 100 ml blue-capped bottle, then add 1 g of titanyl sulfate, stir and ultrasonicate (stir for 2 h, ultrasonicate for 1 h alternately for 3-5 times) to obtain a milky white mixed suspension; then introduce the milky white mixed suspension into a 100 mL polytetrafluoroethylene liner for a sealed solvent thermal reaction for 12 h, and the sealed solvent thermal reaction temperature is 150 ° C. After the reaction is completed, vacuum filtration and alcohol washing (using ethanol for filtration, washing 3 times with 30 ml of ethanol each time) are performed to obtain a white TiO2 solid; then put it into a blast drying oven and dry it overnight, and the temperature of the blast drying oven is 60 ° C, and the drying time is 12 h to obtain a white TiO2 hollow tube powder; 5 g White TiO2 hollow tube powder is put into a quartz boat, which is then put into a quartz tube furnace. High-purity argon gas is first introduced to replace the air in the furnace tube, and then argon gas is introduced and the temperature begins to rise. The argon flow rate is controlled at 50cc, and the heating rate is 5°C / min. The temperature is raised to 550°C and then kept constant at this temperature for 2h to obtain black TiO2 hollow tube powder. In order to produce oxygen vacancies, the black TiO2 hollow tube powder is etched in plasma for 2min at an etching power of 300W to obtain oxygen vacancy-rich TiO2 powder, which is called D-TiO2 hollow nanotube powder.
[0073] Preparation of S2, RuO2 / D-TiO2 catalyst:
[0074] 20 mg of D-TiO2 carrier and 2 ml (10 mg / ml) of RuCl3.XH2O were dispersed in an aqueous solution, and after being uniformly stirred at room temperature for 12 h, they were stirred at 110°C for 12 h, so that the Ru in RuCl3.XH2O was uniformly loaded on the D-TiO2 hollow nanotubes. The solid product was collected by filtration, washed three times with ultrapure water, using 20-50 ml of ultrapure water each time, and dried in vacuum; finally, it was kept warm at 300°C for 2 h in a muffle furnace with a heating rate of 2°C / min.
[0075] Figure 5 Through X-ray diffraction phase analysis (XRD), it was found that D-TnO2 and the standard card PDF-21-1272 of titanium dioxide matched well, proving that the carrier was successfully prepared. Figure 6 Through X-ray diffraction phase analysis (XRD), it was found that RuO2NPs / D-TnO2 matched well with the standard card PDF-21-1272 of titanium dioxide and the standard card PDF-43-1027 of rutile ruthenium dioxide, proving that the catalyst was successfully prepared. Figure 8 Electron paramagnetic resonance (EPR) was used to demonstrate the successful preparation of titanium dioxide oxygen vacancies.
[0076] The morphology of D-TiO2 hollow nanotubes and RuO2 / D-TiO2 catalysts was observed by scanning electron microscopy (SEM). Fig.11 This is the SEM image of D-TiO2 hollow nanotubes. Fig.12 This is the SEM image of RuO2 / D-TiO2 catalyst.
[0077] Comparative Example 1
[0078] The preparation method of the RuO2 / SnO2 catalyst provided in this comparative example specifically comprises the following steps:
[0079] Weigh 20 mg SnO2 carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in an aqueous solution and place them in a 100 ml beaker. After uniformly stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on SnO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml ultrapure water, and dry it in vacuum; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain a RuO2 / SnO2 catalyst.
[0080] Comparative Example 2
[0081] The preparation method of the carbon powder-supported ruthenium oxide catalyst (RuO2 / C) provided in this comparative example specifically comprises the following steps:
[0082] 20 mg of C carrier and 2 ml (10 mg / ml) of RuCl3.XH2O were weighed, dispersed in an aqueous solution and placed in a 100 ml beaker. After uniform stirring at room temperature for 12 hours, the mixture was transferred to a 50 ml round-bottom flask and stirred at 80-120°C for 12 hours to uniformly load Ru in RuCl3.XH2O on C. The solid product was collected by filtration, washed with ultrapure water for 3 times, each time with 20-30 ml of ultrapure water, and dried in vacuo; finally, the mixture was kept warm at 100-400°C for 2-6 hours at a heating rate of 2°C / min in a muffle furnace to obtain a carbon powder-loaded ruthenium oxide catalyst (RuO2 / C).
[0083] Comparative Example 3
[0084] The preparation method of RuO2 / argon D-SnO2 provided in this comparative example specifically comprises the following steps:
[0085] 1. Place 1-5g of light blue SnO2 mineral crystal powder in a tubular furnace, first introduce high-purity argon gas to replace the air in the furnace tube, and then keep it warm for 2-5h at 350-550℃ in an atmosphere of argon and hydrogen mixture (argon and hydrogen flow ratio is 95cc:5cc, argon flow is 95cc, hydrogen flow is 5cc), to obtain oxygen-rich SnO2 mineral crystal powder, called argon D-SnO2 mineral crystal powder;
[0086] 2. Take 20 mg of argon D-SnO2 mineral crystal powder carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in aqueous solution and place them in a 100 ml beaker. After uniform stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on D-SnO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml of ultrapure water, and vacuum dry it; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain RuO2 / argon D-SnO2.
[0087] Comparative Example 4
[0088] The preparation method of RuO2 / argon normal temperature plasma D-SnO2 provided in this comparative example specifically comprises the following steps:
[0089] 1-5g of light blue SnO2 mineral crystal powder is placed in a tubular furnace, high-purity argon gas is introduced to replace the air in the furnace tube, and then the mixture is kept at 350-550°C in an argon and hydrogen mixture atmosphere (argon and hydrogen flow ratio is 95cc:5cc, argon flow is 95cc, hydrogen flow is 5cc) for 2-5h to obtain oxygen-rich SnO2 mineral crystal powder, which is called argon D-SnO2 mineral crystal powder;
[0090] 1-5g of light blue argon D-SnO2 mineral crystal powder was placed in a normal temperature plasma at a power of 300W and kept warm for 2 minutes to obtain argon normal temperature plasma D-SnO2 mineral crystal;
[0091] Take 20 mg of argon room temperature plasma D-SnO2 mineral crystal carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in aqueous solution and place them in a 100 ml beaker. After uniformly stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on D-SnO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml of ultrapure water, and vacuum dry it; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain RuO2 / argon room temperature plasma D-SnO2.
[0092] Comparative Example 5
[0093] The preparation method of RuO2 / argon D-TiO2 provided in this comparative example specifically comprises the following steps:
[0094] 1-5g of light blue TiO2 powder is placed in a tube furnace, high-purity argon gas is introduced to replace the air in the furnace tube, and then the furnace is kept at 350-550℃ in an argon atmosphere for 2-5h to obtain oxygen-rich TiO2 mineral crystal powder, which is called argon D-TiO2 mineral crystal powder;
[0095] Take 20 mg of argon D-TiO2 mineral crystal powder carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in aqueous solution and place them in a 100 ml beaker. After uniformly stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on D-SnO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml of ultrapure water, and vacuum dry it; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain RuO2 / argon D-TiO2.
[0096] Comparative Example 6
[0097] The preparation method of RuO2 / argon hydrogen D-TiO2 provided in this comparative example specifically comprises the following steps:
[0098] 1-5g of light blue TiO2 powder is placed in a high plasma, high-purity argon gas is introduced to replace the air in the furnace tube, and then the temperature is kept at 350-550℃ and argon atmosphere with a heat preservation power of 1000W for 0.5h to obtain oxygen-rich vacancy TnO2 mineral crystal powder, which is called TiO2 mineral crystal powder;
[0099] 1-5g of light blue TiO2 mineral crystal powder is placed in a tube furnace, high-purity argon is introduced to replace the air in the furnace tube, and then the mixture is kept at 350-550°C in an argon and hydrogen mixture atmosphere (the flow ratio of argon and hydrogen is 95cc:5cc, the argon flow is 95cc, and the hydrogen flow is 5cc) for 2-5h to obtain oxygen-rich TiO2 mineral crystal powder, which is called argon hydrogen D-TiO2 powder;
[0100] Take 20 mg of argon hydrogen D-TiO2 powder carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in an aqueous solution and place them in a 100 ml beaker. After uniformly stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on the argon hydrogen D-TiO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml of ultrapure water, and vacuum dry it; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain RuO2 / argon hydrogen D-TiO2.
[0101] Comparative Example 7
[0102] Commercial RuO2 catalyst. Ruthenium(IV)oxide Molecular formula: RuO2; CAS number: 12036-10-1; MDL number: MFCD00011210.
[0103] Comparative Example 8
[0104] The preparation method of the RuO2 / TiO2 catalyst provided in this comparative example specifically comprises the following steps:
[0105] Weigh 20 mg TiO2 carrier and 2 ml (10 mg / ml) RuCl3.XH2O, disperse them in an aqueous solution and place them in a 100 ml beaker. After uniformly stirring at room temperature for 12 hours, transfer them to a 50 ml round-bottom flask and stir them at 80-120°C for 12 hours to make the Ru in RuCl3.XH2O uniformly loaded on TiO2. Collect the solid product by filtration, wash it with ultrapure water for 3 times, each time with 20-30 ml ultrapure water, and dry it in vacuum; finally, keep it in a muffle furnace at 100-400°C for 2-6 hours at a heating rate of 2°C / min to obtain a RuO2 / TiO2 catalyst.
[0106] Anode oxygen evolution performance test example
[0107] A three-electrode system was used to perform linear scan tests in 0.5 M H2SO4 saturated with oxygen at a scan rate of 5 mV / s.
[0108] Fig.14The OER polarization curves of the RuO2 / D-SnO2 catalyst prepared in Example 1, the RuO2 / SnO2 prepared in Comparative Example 1, the carbon powder supported ruthenium oxide catalyst (C / RuO2) prepared in Comparative Example 2, and the commercial RuO2 catalyst in Comparative Example 7 in 0.5M H2SO4 are shown. Fig.14 It can be seen from the polarization curve that the catalyst prepared in Example 1 exhibits oxygen evolution performance superior to that of the catalyst in the comparative example.
[0109] Fig.16 The RuO2 / D-SnO2 catalyst prepared in Example 1, the RuO2 / argon D-SnO2 catalyst prepared in Comparative Example 3, and the RuO2 / argon D-SnO2 catalyst prepared in Comparative Example 4 are shown. 2 / OER polarization curves of different D-SnO2 catalysts in 0.5M H2SO4 under argon plasma at room temperature. Fig.16 It can be seen that the stronger the oxygen vacancy signal of the carrier, the better the performance after loading the precious metal.
[0110] A three-electrode system was used to perform linear scan tests in 0.5 M H2SO4 saturated with oxygen at a scan rate of 5 mV / s.
[0111] Fig.15 The OER polarization curves of the RuO2 / D-TiO2 catalyst prepared in Example 2, the RuO2 / TiO2 prepared in Comparative Example 8, the C / RuO2 prepared in Comparative Example 2, the D-TiO2 prepared in Example 2, and the commercial RuO2 catalyst in Comparative Example 7 in 0.5M H2SO4 are shown. Fig.15 It can be seen from the polarization curve that the catalyst prepared in Example 2 exhibits oxygen evolution performance superior to that of the catalyst in the comparative example.
[0112] Fig.17 The RuO2 / D-TiO2 catalyst prepared in Example 2 and the RuO2 / D-TiO2 catalyst prepared in Comparative Example 5 are shown. 2 / The OER polarization curves of the argon D-TiO2 catalyst and the RuO2 / argon hydrogen D-TiO2 catalyst prepared in Comparative Example 6 in 0.5M H2SO4 are shown in Figure 2. Fig.17 It can be seen that the stronger the oxygen vacancy signal of the carrier, the better the performance after loading the precious metal.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing an oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst, It is characterized in that The following steps are involved: S1, dissolving a ruthenium source and an oxygen vacancy-rich oxide carrier in water, stirring evenly at room temperature to obtain a mixed solution; S2, heating and stirring the mixed solution to obtain a black suspension, and filtering, washing, and drying the black suspension to obtain a precursor solid; S3, calcining the precursor solid to obtain an oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst.
2. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 1, It is characterized in that In step S1, the ruthenium source is RuCl 3 .XH 2 O,RuCl 3 .XH 2 The dosage ratio of O and oxygen-rich vacancy oxide is (1-20 mg): 20 mg; or In step S1, the stirring time at room temperature is 10-15h; or In step S2, the heating and stirring temperature is 80-120° C., and the heating and stirring time is 12 h; or In step S3, the specific calcination conditions are: placing in a muffle furnace under air atmosphere at a temperature of 100-400° C. at a heating rate of 2° C. / min for 2-6 hours.
3. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 1, It is characterized in that In step S2, the specific washing conditions are: washing by suction filtration, the number of washing times is 3-5 times, the detergent is ultrapure water, and 15-50 ml is used each time; or In step S2, the specific drying conditions are: placing in a blast drying oven and drying overnight, the temperature of the drying oven is 60-120°C, the drying time is 8-12h, or the drying is vacuum drying.
4. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 1, It is characterized in that When the oxygen-vacancy-rich oxide is oxygen-vacancy-rich SnO 2 When the oxygen-rich SnO 2 The preparation process is: Tin chloride pentahydrate, ethanol, ultrapure water and sodium hydroxide were mixed, stirred and ultrasonically treated to obtain a white mixed suspension; the white mixed suspension was then subjected to a sealed solvent thermal reaction at a temperature of 180-220°C for 24 hours, and after the reaction was completed, the mixture was centrifuged and washed with ultrapure water to obtain SnO 2 Light blue solid powder; then SnO 2 The light blue solid powder was dried at 60-120℃ for 8-12h to obtain light blue SnO 2 Mineral crystal powder; light blue SnO 2 The mineral powder was heated at 350-550℃ for 2-5h in a mixed atmosphere of argon and hydrogen to create oxygen vacancies and obtain oxygen-rich SnO 2 Mineral powder, marked as D-SnO 2 Mineral crystal powder.
5. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 4, It is characterized in that The dosage ratio of tin chloride pentahydrate, ethanol, ultrapure water and sodium hydroxide is 1.33g:(25ml-30ml):(25ml-30ml):1.26g, wherein the volume ratio of ultrapure water to ethanol is 1:1; or The specific process of the stirring and ultrasonic treatment is: ultrasonic treatment for 0.5 h and stirring for 1 h are performed alternately 3-5 times.
6. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 4, It is characterized in that The specific conditions of the centrifugation and ultrapure water washing are: washing after the reaction is completed and centrifuging with ultrapure water, washing 4-6 times with 20-30 ml of ultrapure water each time, the washing speed is 1200 r / min, and the washing time for each time is 10 min; or The flow ratio of argon gas to hydrogen gas is 95:5, the flow rate of argon gas is 95cc, and the flow rate of hydrogen gas is 5cc.
7. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 1, It is characterized in that When the oxygen-vacancy-rich oxide is oxygen-vacancy-rich TiO 2 When the oxygen-rich TiO 2 The preparation process is: Titanyl sulfate, ethanol, ether and glycerol were mixed, stirred and ultrasonically treated to obtain a milky white mixed suspension; the milky white mixed suspension was then subjected to a sealed solvent thermal reaction at a temperature of 100-150°C for 12 hours, and after the reaction was completed, vacuum filtration and alcohol washing were performed to obtain TiO 2 White solid; then dried overnight at 60-80°C to obtain white TiO 2 Hollow tube powder; white TiO 2 The hollow tube powder was calcined at 550 °C for 2-5 h in an argon atmosphere to obtain black TiO 2 Hollow tube powder; black TiO 2 The hollow tube powder was etched in plasma for 1-3 min to create oxygen vacancies. The etching power was 300-600 W to obtain oxygen-rich TiO 2 Powder, denoted as D-TiO 2 Hollow nanotube powder.
8. The method for preparing the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 7, It is characterized in that The titanyl sulfate, ethanol, ether and glycerol are used in a ratio of 1 g: (25 ml-30 ml): (15 ml-18 ml): (15 ml-18 ml); or The stirring and ultrasonic treatment specifically includes: stirring for 2 hours and ultrasonic treatment for 1 hour, alternately for 3-5 times; or The vacuum filtration and alcohol washing specifically include: washing the white solid obtained by the thermal reaction of the sealed solvent, filtering with ethanol, and washing 4-6 times with 20-50 ml of ethanol each time.
9. An oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst, It is characterized in that An oxygen-rich vacancy oxide-loaded noble metal ruthenium dioxide catalyst prepared by the method described in any one of claims 1 to 8.
10. Use of the oxygen-rich vacancy oxide-supported noble metal ruthenium dioxide catalyst according to claim 9 in electrolysis of water.
Citation Information
Cited By
Montmorillonite-loaded ruthenium oxide catalyst as well as preparation method and application thereof
CN119663367A