Fenton iron peat-based MoO2 heterogeneous Fenton-like catalyst as well as preparation method and application of Fenton iron peat-based MoO2 heterogeneous Fenton-like catalyst
By preparing Fenton iron peat-based @MoO2 heterophase Fenton catalyst, the problems of narrow pH range and large iron sludge generation in traditional Fenton reactions were solved, and efficient treatment of difficult-to-degrade organic pollutants at neutral pH was achieved. , reduces costs and improves the efficiency of catalyst recycling.
Patent Information
- Application Number
- CN202411040006.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional Fenton reaction has problems such as narrow pH range, large iron sludge generation, difficulty in recycling catalysts and high cost in the treatment of difficult-to-degrade organic pollutants in water bodies.
Using the preparation method of Fenton iron peat-based @MoO2 heterophasic Fenton catalyst, a mixture of Fenton iron sludge and ammonium molybdate tetrahydrate and high-temperature pyrolysis treatment was prepared to prepare a kind of capable of under neutral pH conditions. The working catalyst uses MoO2 as a cocatalyst to improve the reaction rate and the cycling efficiency of the catalyst.
The reaction pH range is broadened, the dosage of drugs is reduced, the cost is reduced, the catalyst is easily recovered and resource-based, the COD treatment effect is improved, the generation of iron sludge is avoided, and the sludge treatment cost is reduced.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to a heterogeneous Fenton-type catalyst, and more specifically to a Fenton iron peat-based @MoO2 heterogeneous Fenton-type catalyst and a preparation method and application thereof, belonging to the technical field of catalysts. Background Art
[0002] For the sustainable development of human society and ecological environment, the removal of refractory organic pollutants in water bodies is urgent. At present, the main treatment methods for refractory organic matter in water bodies include physical method, chemical method, biological method, advanced oxidation method, etc. Among them, the advanced oxidation method mainly realizes the mineralization of organic matter through active free radicals such as hydroxyl free radicals, which has the advantages of simple operation, thorough mineralization and high removal efficiency. Fenton technology is the earliest invented advanced oxidation technology and is also the most widely used advanced oxidation technology. This technology is an economical and efficient wastewater treatment technology with the advantages of strong oxidizability, low cost, and operation under normal temperature and pressure conditions. It is widely used in textile, pharmaceutical, papermaking, garbage disposal, chemical and other industries.
[0003] The Fenton process is generally a reaction of hydrogen peroxide with iron ions in an acidic medium to produce a strong oxidant, namely hydroxyl radicals, which have strong oxidizing properties and can mineralize pollutants into carbon dioxide and water.
[0004] However, in the traditional Fenton reaction, the pH value of the reaction system directly affects the hydrolysis form of iron. When the pH value is greater than 3, a large amount of iron ions in the solution will form precipitation, affecting the progress of the Fenton reaction. Therefore, the traditional Fenton reaction has a high pH value requirement for the reaction solution, and a large amount of iron sludge will be formed during the reaction. In addition, during the reaction, H2O2 may react with Fe 3+ Reaction and Fe 2+ The deficiency leads to its low utilization rate and insufficient subsequent degradation of pollutants, which greatly limits the application of Fenton reaction in wastewater treatment.
[0005] The traditional Fenton method has several obvious disadvantages: (1) the reaction pH range is narrow, and the pH value is generally adjusted to 2-3 to prevent the formation of iron hydroxide precipitation; (2) Fe 3+ Conversion to Fe 2+ It is the rate-limiting step in the entire reaction, which reduces the reaction rate; (3) Fe 2+ It is difficult to separate from water, which limits the recycling of the catalyst and leads to a large waste of resources; (4) high cost; (5) large amount of iron sludge, etc. Summary of the invention
[0006] The purpose of the present invention is to provide a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst and its preparation method and application, so as to solve the technical problems of narrow pH value range, large H2O2 consumption and easy generation of large amount of iron mud in traditional Fenton application.
[0007] To achieve the above object, the present invention provides a method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst, comprising the following steps:
[0008] Step 1: pre-treating Fenton iron mud;
[0009] Step 2: Grind the pretreated Fenton iron mud and ammonium molybdate tetrahydrate in a mortar and mix them evenly;
[0010] Step 3: Place the Fenton iron mud and ammonium molybdate tetrahydrate mixed in step 2 in a tubular furnace, perform high-temperature pyrolysis treatment under inert gas protection, and naturally cool to room temperature after high-temperature pyrolysis treatment to obtain the Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst.
[0011] Furthermore, in step 1, the Fenton iron mud contains iron hydroxide and iron oxyhydroxide; wherein the mass fraction of iron element is greater than 20%, and the mass fraction of carbon element is greater than 20%.
[0012] Furthermore, in step one, the Fenton iron mud is pretreated, specifically, the Fenton iron mud is placed in a 60-105° C. constant temperature drying oven for drying (water content <10%) and grinding.
[0013] Furthermore, in step 1, the dried and ground Fenton iron mud is passed through a 10-1000 mesh standard sieve, and the sieve residue is the pretreated Fenton iron mud.
[0014] Furthermore, in step 2, the mass ratio of the pretreated Fenton iron mud to ammonium molybdate tetrahydrate is 3.5-10.7:1.
[0015] Furthermore, in step three, the high temperature pyrolysis treatment is specifically: heating to 300-800° C. at a heating rate of 2-20° C. / min and maintaining for 1-3 hours.
[0016] Furthermore, in step three, the inert gas is nitrogen or argon.
[0017] The present invention also provides a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst, and the Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst is prepared by the above-mentioned preparation method.
[0018] The present invention also provides a Fenton iron peat-based @MoO2 heterogeneous Fenton catalyst prepared by the above-mentioned preparation method or the use of the above-mentioned Fenton iron peat-based @MoO2 heterogeneous Fenton catalyst in the treatment of difficult-to-degrade organic pollutants using heterogeneous Fenton technology.
[0019] The present invention has the following beneficial effects:
[0020] (1) Iron ions will generate precipitation and mix it into sludge under neutral or alkaline conditions to form Fenton iron sludge. Sludge contains high concentrations of iron oxides, a small amount of organic matter and some heavy metals. If it is directly discharged, it will seriously damage the ecological environment. The present invention realizes waste treatment by preparing iron sludge into a heterogeneous Fenton catalyst, achieves the purpose of resource utilization of Fenton iron sludge, and avoids the subsequent generation of iron sludge.
[0021] (2) The traditional Fenton reaction has a narrow pH range, usually controlled at 2-3, and requires the addition of a large amount of reagents. The present invention introduces a heterogeneous Fenton catalyst to broaden the reaction pH threshold, increase the applicability of the catalyst, reduce the amount of reagents used, and reduce costs. Because the traditional Fenton reaction is under acidic conditions, ferrous ions and hydrogen peroxide produce hydroxyl radicals. Adjusting to acidity prevents ferrous ions and ferric ions from forming precipitation, which affects the generation of hydroxyl radicals. The catalyst prepared by the present invention is a heterogeneous Fenton reaction, the essence of which is that H2O2 molecules generate hydroxyl radicals on the surface of a solid catalyst. The heterogeneous Fenton reaction process of the catalyst prepared by the present invention includes the following steps: organic pollutants diffuse to the catalyst surface and form bonds with the active centers on the catalyst surface (i.e., specific adsorption on the reaction site); electrons migrate to the active sites of the adsorbed organic matter, and the organic matter dissociates and the reaction sites regenerate subsequently. The reaction can be carried out at a neutral pH, eliminating the acidification and neutralization steps, thereby avoiding the formation of iron sludge. At the same time, the catalyst is easy to recover and regenerate, simplifying the operation in wastewater treatment.
[0022] (3) Fe in traditional Fenton reaction 3+ Conversion to Fe 2+ It is the rate-limiting step in the entire reaction, which reduces the reaction rate. In the present invention, MoO2 can be used as a co-catalyst to enhance the Fe 3+ / Fe 2+ The cycle efficiency is improved, the catalyst stability is improved and it can be reused. Because the low-coordinated oxygen on the surface of MoO2 can capture protons to form water and expose the metal reduction active site Mo 4+ , Fe 3+ Reduction to Fe 2+ , thus significantly improving the reaction rate of the rate-limiting step in the traditional Fenton reaction. The H2O2 in the Fenton reaction further converts Mo 6+ Restore to Mo 4+Complete the MoO2 catalytic cycle. In the catalytic process, the Fenton reagent H2O2 and Fe 2+ The usage of (catalyst) is of great significance to reduce iron sludge pollution and lower reagent costs.
[0023] (4)Fe 2+ It is difficult to separate from water, which limits the recycling of the catalyst and leads to a large waste of resources. The magnetic catalyst prepared by the present invention is easy to recycle and realizes the repeated use of the catalyst. 2+ It exists in the solution in an ionic state, and it is difficult to directly separate it. It is precipitated by other means. Due to the change of its valence state and form, there is no catalytic effect, and it needs to be further reacted by other chemical methods, and the steps are cumbersome and the cost is high. The heterogeneous Fenton catalyst prepared by the present invention presents a solid particle state, which is essentially different from the ferrous ion in the dissolved state in form, and the separation difficulty is small. In addition, ferrosoferric oxide is magnetic, so the catalyst can be carried out by magnetic separation.
[0024] (5) Compared with the traditional Fenton agent ferrous sulfate, the Fenton iron peat-based @MoO2 heterogeneous Fenton catalyst provided by the present invention can improve the COD treatment effect by 30%, greatly reduce the treatment cost, and has good potential for industrial application.
[0025] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention will be further described in detail below. DETAILED DESCRIPTION
[0026] The following is a detailed description of embodiments of the present invention, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0027] Fenton iron mud has certain toxicity and is generally considered as hazardous waste. If it is not properly disposed of, it will cause secondary pollution and waste resources. In some areas, the cost of treating Fenton iron mud has reached 2,000-3,000 yuan / t. At present, the main treatment process of Fenton iron mud is dehydration, thermal drying, incineration, and landfill disposal. However, the traditional landfill method has poor treatment effect on Fenton iron mud and occupies a large amount of land; stacking Fenton iron mud with high water content will produce odor and produce leachate that will destroy soil structure and endanger human health; Fenton iron mud has a low calorific value and is easy to coke after incineration, affecting the normal operation of the incinerator.
[0028] Pyrolysis carbonization technology can remove organic pollutants in sludge, kill pathogenic microorganisms, solidify sludge organic matter and heavy metals, and prepare carbon-based functional materials to achieve harmless and resource-based utilization of sludge.
[0029] The main components of Fenton iron sludge are iron hydroxide and iron oxide. The mass fraction of iron-containing compounds in the iron sludge is 40%-60%. The element composition content of Fenton sludge produced by different types of sewage projects (papermaking wastewater, pulping and papermaking wastewater, landfill leachate, etc.) treated with Fenton technology will be different.
[0030] Landfill leachate refers to highly polluted wastewater generated during the landfill or stacking of urban domestic waste due to atmospheric precipitation, water produced by the decomposition of degradable organic matter by microorganisms, and water carried by the waste itself. The sources of water in leachate are mainly the following: (1) atmospheric precipitation, mainly including precipitation and snowfall; (2) surface runoff and inflow of irrigation water; (3) groundwater infiltration, groundwater infiltration into landfills with inadequate anti-seepage measures; (4) water carried by the waste itself and water produced by decomposition. Garbage with a high water content, such as kitchen waste, is squeezed or decomposed by microorganisms in the landfill, thereby releasing water to produce landfill leachate.
[0031] When the type of garbage treated in the landfill is domestic garbage with a high water content, the leachate produced not only has a high organic matter content, but also a large amount.
[0032] Because carbon, as a carrier in the catalyst, can provide attachment sites for iron-containing compounds (catalyst active substances), thereby increasing the use efficiency of the catalyst. The project type of Fenton sludge selected in the embodiments and comparative examples of the present invention is: iron sludge generated by the project of treating landfill leachate using Fenton technology. The mass fraction of iron in the iron sludge is 20%-30%, and the mass fraction of carbon is 20%-30%. The carbon content is high, and the pyrolysis carbonization product has good performance.
[0033] Under neutral or alkaline conditions, iron ions will generate precipitation and mix it into sludge to form Fenton iron sludge. Sludge contains high concentrations of iron oxides, a small amount of organic matter and some heavy metals. If it is directly discharged, it will seriously damage the ecological environment. The present invention realizes waste treatment by preparing iron sludge into a heterogeneous Fenton catalyst, achieves the purpose of resource utilization of Fenton iron sludge, and avoids the subsequent generation of iron sludge.
[0034] The present invention is explained below with reference to specific embodiments.
[0035] Embodiment 1:
[0036] A Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst and a preparation method thereof, comprising the following steps:
[0037] (1) Take 500g of Fenton iron mud from the landfill leachate project, put it into a 60-105℃ constant temperature drying oven for drying, until the weight is stable within 1g, indicating that the drying is complete, grind it with an agate mortar, and pass it through a 10-1000 mesh laboratory standard sieve, take the sieve, collect it in a sealed bag for use, and obtain FS powder. Among them, the moisture in the sludge is dried to remove the influence of oxygen on the pyrolysis process. After drying, the sludge will form large lumps. After grinding, the sludge and ammonium molybdate are fully mixed, which is beneficial to the doping effect of molybdenum. In addition, the powder is beneficial to the sufficiency of the pyrolysis process. In addition, the larger the mesh number, the finer the powder, the finer the catalyst, the more sufficient the contact with the pollutant, and the higher the reaction efficiency.
[0038] (2) Take 50g FS powder and 5g ammonium molybdate tetrahydrate and put them in a mortar with a mass ratio of FS powder to ammonium molybdate tetrahydrate of 10:1. Grind for 30min to mix them thoroughly and transfer them to a porcelain boat.
[0039] (3) Then the porcelain boat is placed in a tube furnace, and under nitrogen protection, heated to 700°C at a heating rate of 2-20°C / min and maintained for 1-3 hours, and naturally cooled to room temperature to obtain FSC@MoO2. The main components of FSC@MoO2 are Fe3O4 (content 40%-60%), MoO2, Fe2O3, C and Fe 0 .
[0040] Embodiment 2:
[0041] A Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst and a preparation method thereof, comprising the following steps:
[0042] (1) Take 500 g of Fenton iron mud from the landfill leachate project, put it into a constant temperature drying oven at 60-105°C and dry it until the weight is stable within 1 g, indicating that the drying is complete. Grind it with an agate mortar and pass it through a 10-1000 mesh laboratory standard sieve. Collect the sieved material in a sealed bag for later use to obtain FS powder.
[0043] (2) 17.6 g FS powder and 5 g ammonium molybdate tetrahydrate were placed in a mortar with a mass ratio of FS powder to ammonium molybdate tetrahydrate of 3.5:1. Grind for 30 min to mix thoroughly and transfer to a porcelain boat.
[0044] (3) The porcelain boat is then placed in a tube furnace and heated to 300°C at a heating rate of 2-20°C / min under nitrogen protection and maintained for 1-3 h, and then naturally cooled to room temperature to obtain FSC@MoO2.
[0045] Embodiment 3:
[0046] A Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst and a preparation method thereof, comprising the following steps:
[0047] (1) Take 500 g of Fenton iron mud from the landfill leachate project, put it into a constant temperature drying oven at 60-105°C and dry it until the weight is stable within 1 g, indicating that the drying is complete. Grind it with an agate mortar and pass it through a 10-1000 mesh laboratory standard sieve. Collect the sieved material in a sealed bag for later use to obtain FS powder.
[0048] (2) 53.1 g FS powder and 5 g ammonium molybdate tetrahydrate were placed in a mortar with a mass ratio of FS powder to ammonium molybdate tetrahydrate of 10.7:1. Grind for 30 min to mix thoroughly and transfer to a porcelain boat.
[0049] (3) The porcelain boat was then placed in a tube furnace and heated to 800 °C at a heating rate of 2-20 °C / min under nitrogen protection and maintained for 1-3 h, and then naturally cooled to room temperature to obtain MoO2@FSC.
[0050] Comparative Example 1: (Ammonium molybdate tetrahydrate content is too high)
[0051] The difference between Comparative Example 1 and Example 1 is that in step (2), the mass ratio of FS powder to ammonium molybdate tetrahydrate is 3:1, and the rest is the same as Example 1.
[0052] Comparative Example 2: (Ammonium molybdate tetrahydrate content is too low)
[0053] The difference between Comparative Example 2 and Example 1 is that in step (2), the mass ratio of FS powder to ammonium molybdate tetrahydrate is 12:1, and the rest is the same as Example 1.
[0054] Comparative Example 3: (pyrolysis temperature is too high)
[0055] The difference between Comparative Example 3 and Example 1 is that in step (3), the temperature is raised to 900° C., and the rest is the same as Example 1.
[0056] Comparative Example 4: (pyrolysis temperature is too low)
[0057] The difference between Comparative Example 4 and Example 1 is that in step (3), the temperature is raised to 250° C., and the rest is the same as Example 1.
[0058] The Fenton-like catalyst prepared by the present invention is applied to the treatment of water containing refractory organic pollutants. The FSC@MoO2 catalyst prepared in Example 1 of the present invention and the catalyst prepared in Comparative Examples 1-4 were used to conduct a comparative stirring experiment with conventional reagent ferrous sulfate, and a comparative analysis was conducted from aspects such as COD treatment effect, sludge production, dosage, and pH range. Specifically, the biochemical effluent of the landfill leachate project was used for the experiment. The water quality of the biochemical effluent of the landfill leachate project is shown in Table 1.
[0059] Table 1:
[0060] Water quality type COD pH Biochemical effluent 721mg / L 7.8
[0061] Comparative experiments were conducted using the FSC@MoO2 catalyst prepared in Example 1 of the present invention, the catalysts prepared in Comparative Examples 1-4, and conventional agent ferrous sulfate to compare and analyze the biochemical effluent in terms of pH, sludge production, and COD treatment effect. The experimental results are shown in Table 2.
[0062] Table 2:
[0063]
[0064]
[0065] It can be seen from Table 2 that when COD treatment is carried out under the same conditions, the COD removal rate of the catalyst prepared in Example 1 is 82.9%, the COD removal rate of the catalyst prepared in Comparative Example 1 is 63.5%, the COD removal rate of the catalyst prepared in Comparative Example 2 is 59.3%, the COD removal rate of the catalyst prepared in Comparative Example 3 is 68.2%, and the COD removal rate of the catalyst prepared in Comparative Example 4 is 65.8%.
[0066] By comparing Example 1 with Comparative Example 1 and Comparative Example 2, it can be seen that: when the content of ammonium molybdate tetrahydrate is too high, or the content of ammonium molybdate tetrahydrate is too low, the catalyst effect obtained is not as good as the catalyst effect obtained in Example 1. This is because the iron content in the Fenton iron sludge of the landfill leachate project is 20%-30%, and the Fenton reaction effects of composite catalysts with different Mo / Fe molar ratios are different. Mo is used as a co-catalyst. A low content will lead to weak catalytic degradation activity, and a high content will lead to a certain antagonistic effect with Fe. Therefore, the two can only produce good synergistic effects within a suitable molar ratio range. The suitable molar ratio range of Mo / Fe is 0.05-0.15. The low-coordinated oxygen on the surface of MoO2 can capture protons to form water and expose the metal reduction active site Mo. 4+ , Fe 3+ Reduction to Fe 2+ , thus significantly improving the reaction rate of the rate-limiting step in the traditional Fenton reaction. The H2O2 in the Fenton reaction further converts Mo 6+ Restore to Mo 4+ Complete the MoO2 catalytic cycle. In the catalytic process, the Fenton reagent H2O2 and Fe 2+ The amount of (catalyst) used is of great significance to reduce iron sludge pollution and reduce reagent costs. The release of toxic H2S in the process of MoS2 catalyzing Fenton or Fenton-like reactions is a disadvantage of the system, so MoO2 has more advantages such as green, non-toxic and high efficiency.
[0067] By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that when the pyrolysis temperature is too high or too low, the catalyst effect obtained is not as good as the catalyst effect obtained in Example 1. This is because pyrolysis technology refers to the technology of converting sludge into bio-oil, biogas and biochar by high-temperature decomposition in the absence of oxygen or inert gas. Temperature is an important factor affecting the specific surface area and pore volume of biochar obtained by sludge pyrolysis. During the pyrolysis process, the continuous decomposition of organic matter releases gas and bio-oil vapor, which forms many pore structures on the surface of the solid product. However, if the pyrolysis temperature is too high, the organic matter will be over-decomposed, resulting in the collapse of the pore structure of the solid product, the reduction of the specific surface area, and the reduction of active sites, which leads to a decrease in the catalytic effect. If the pyrolysis temperature is too low, the pyrolysis will be incomplete, the pore structure will not be completely released, the specific surface area will be small, the carbonization will not be complete, and the active sites will be reduced, resulting in a decrease in the catalytic effect.
[0068] By comparing Example 1 with the conventional reagent ferrous sulfate, it can be seen that for the traditional homogeneous Fenton reaction, it is necessary to adjust the pH by adding acid so that the pH range of the system is controlled at 2-3, while for the heterogeneous system (the present invention), the most suitable pH range is 4-6, indicating that the amount of acid and alkali reagent added in the heterogeneous system (heterogeneous catalyst) is less than that in the homogeneous system (adding ferrous sulfate), which can reduce the use of reagents, save costs, and have economic advantages. In addition, due to the doping of MoO2, the Fe in the Fenton reaction is strengthened. 3+ / Fe 2+ The cycle efficiency is improved, and the ability of catalyst recycling is enhanced. The COD removal rate of the heterogeneous system is about 30.8% higher than that of the homogeneous system; finally, the heterogeneous system (adding heterogeneous catalysts) produces almost no sludge, while the homogeneous system (adding ferrous sulfate) produces a large amount of iron sludge, and 7.93 kg of Fenton iron sludge is produced per ton of water treated. Therefore, the present invention does not incur additional sludge treatment costs, and can make resource utilization of sludge produced by traditional Fenton processes in other landfill leachate projects. The catalysts prepared in Examples 2 and 3 have similar effects to those prepared in Example 1, and will not be repeated here.
[0069] From the above comparison, it can be seen that the catalyst prepared by the present invention reduces the generation of sludge during use, has a wider pH range in the reaction process, reduces the cost of using acid and alkali agents during sewage treatment, and has a better effect on sewage treatment.
[0070] In summary, the present invention provides a method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst, which broadens the reaction pH threshold, increases the applicability of the catalyst, reduces the dosage of the reagent, and reduces the cost by introducing a heterogeneous Fenton-like catalyst. The catalyst prepared by the present invention is a heterogeneous Fenton-like reaction, the essence of which is that H2O2 molecules generate hydroxyl radicals on the surface of a solid catalyst. The heterogeneous Fenton reaction process includes the following steps: organic pollutants diffuse to the catalyst surface and form bonds with the active centers on the surface of the catalytic material (i.e., specific adsorption on the reaction site); electrons migrate to the active sites of the adsorbed organic matter, followed by the dissociation of the organic matter and the regeneration of the reaction site. The reaction can be carried out at a neutral pH, eliminating the acidification and neutralization steps, thereby avoiding the formation of iron sludge. At the same time, the catalyst is easy to recover and regenerate, simplifying the operation in wastewater treatment.
[0071] At the same time, MoO2 in the present invention is used as a co-catalyst to enhance the Fe 3+ / Fe 2+ The cycle efficiency is improved, the catalyst stability is improved and it can be reused. Because the low-coordinated oxygen on the surface of MoO2 can capture protons to form water and expose the metal reduction active site Mo 4+ , Fe 3+ Reduction to Fe 2+ , thus significantly improving the reaction rate of the rate-limiting step in the traditional Fenton reaction. The H2O2 in the Fenton reaction further converts Mo 6+ Restore to Mo 4+ Complete the MoO2 catalytic cycle. In the catalytic process, the Fenton reagent H2O2 and Fe 2+ The amount of catalyst used is of great significance for reducing iron mud pollution and reducing reagent costs. Moreover, the heterogeneous Fenton catalyst prepared by the present invention is in the form of solid particles, which is essentially different from dissolved ferrous ions in form and has little difficulty in separation. In addition, ferroferric oxide is magnetic, so the catalyst can be separated by magnetic separation.
[0072] In addition, iron ions will generate precipitation and mix into the sludge under neutral or alkaline conditions to form Fenton iron sludge. The sludge contains high concentrations of iron oxides, a small amount of organic matter and some heavy metals. If it is directly discharged, it will seriously damage the ecological environment. The present invention realizes waste treatment by preparing iron sludge into a heterogeneous Fenton catalyst, achieves the purpose of resource utilization of Fenton iron sludge, and avoids the subsequent generation of iron sludge.
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst, characterized in that: The following steps are involved: Step 1: pre-treating Fenton iron mud; Step 2: Grind the pretreated Fenton iron mud and ammonium molybdate tetrahydrate in a mortar and mix them evenly; Step 3: Place the Fenton iron mud and ammonium molybdate tetrahydrate mixed in step 2 in a tubular furnace, perform high-temperature pyrolysis treatment under inert gas protection, and naturally cool to room temperature after high-temperature pyrolysis treatment to obtain the Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst.
2. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 1, characterized in that: In step 1, the Fenton iron mud contains iron hydroxide and iron oxyhydroxide; wherein the mass fraction of iron element is more than 20%, and the mass fraction of carbon element is more than 20%.
3. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 1, characterized in that: In step 1, the Fenton iron mud is pretreated, specifically: the Fenton iron mud is placed in a 60-105°C constant temperature drying oven for drying and grinding.
4. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 3, characterized in that: In step 1, the dried and ground Fenton iron mud is passed through a 10-1000 mesh standard sieve, and the sieve residue is the pretreated Fenton iron mud.
5. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 1, characterized in that: In step 2, the mass ratio of the pretreated Fenton iron mud to ammonium molybdate tetrahydrate is 3.5-10.7:
1.
6. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 1, characterized in that: In step three, the high temperature pyrolysis treatment is specifically: heating to 300-800°C at a heating rate of 2-20°C / min and maintaining for 1-3h.
7. The method for preparing a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst according to claim 1, characterized in that: In step three, the inert gas is nitrogen or argon.
8. A Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst, characterized in that: The Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst is prepared by the preparation method described in any one of claims 1-7.
9. Use of a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst prepared by the preparation method described in any one of claims 1 to 7 or a Fenton iron peat-based @MoO2 heterogeneous Fenton-like catalyst described in claim 8 in the treatment of refractory organic pollutants using heterogeneous Fenton technology.
Citation Information
Patent Citations
Preparation method and application of Fenton sludge-based magnetic biochar catalytic material
CN115888712A
MoO2 (iron)-carbon-based composite catalytic material for efficiently and stably removing organic pollutants as well as preparation method and application of MoO2 (iron)-carbon-based composite catalytic material
CN117463353A
Cited By
Method for preparing catalyst based on Fenton iron sludge and activated sludge, prepared catalyst and application