Preparation method and application of N-ZnO / Ti3C2 photocatalyst

By preparing N-ZnO/Ti3C2 photocatalysts, using doped N and composite Ti3C2 to improve the photocatalytic performance, the problem of limited degradation rate and secondary pollution of tetracycline antibiotics in the prior art is solved, and efficient and safe photocatalysis is achieved Degradation effect.

CN118925769APending Publication Date: 2024-11-12GUANGDONG UNIV OF EDUCATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410912416.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When degrading tetracycline antibiotics, the degradation rate is easily limited by pesticide concentration and has the risk of secondary pollution. There is a lack of efficient, stable and difficult to cause pollution.

Method used

Using the preparation method of N-ZnO/Ti3C2 photocatalyst, ZIF-L precursor is prepared by zinc salt and 2-methylimidazole to recombinate with Ti3C2, and calcined to prepare N-ZnO/Ti3C2 photocatalyst, and the photo is improved by doping N-co-combining Ti3C2. Catalytic performance enhances the adsorption and photocatalytic degradation of tetracycline antibiotics.

Benefits of technology

The photocatalytic efficiency and adsorption performance of the photocatalyst are improved, and the degradation rate is significantly improved. The material itself does not change or lose, making it safe and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925769A_ABST
    Figure CN118925769A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of photocatalysis, and discloses a preparation method and application of an N-ZnO / Ti3C2 photocatalyst. The preparation method comprises the following steps: preparing a precursor ZIF-L of N-ZnO from zinc salt and 2-methylimidazole (MIM), etching Ti3AlC2 to obtain multiple layers of Ti3C2, and further calcining the ZIF-L / Ti3C2 compound to prepare the N-ZnO / Ti3C2 photocatalyst. The N-ZnO / Ti3C2 catalyst prepared by the preparation method disclosed by the invention has excellent adsorption performance and photocatalytic degradation performance on tetracycline antibiotics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photocatalysis, and particularly relates to a preparation method and application of an N-ZnO / Ti3C2 photocatalyst. Background Art

[0002] In recent years, antibiotics have been used in various fields, and tetracycline antibiotics are the most widely used. However, their irregular use will lead to the deterioration of the ecological environment, and in severe cases will threaten the health of animals, plants and humans.

[0003] In the process of degrading tetracycline (TC) antibiotics, how to choose an efficient, mature, stable, and non-secondary pollution-prone method for degrading tetracycline antibiotics and a suitable degradation material has become a question worth considering.

[0004] At present, the mainstream methods for TC degradation mainly include adsorption method that relies on electrostatic effect to remove TC, microbial method that uses organisms to degrade antibiotics into small molecule compounds, chemical method, etc. The chemical methods mainly include electrochemical method, advanced oxidation method, photochemical degradation, etc. This method is economical, convenient, relatively mature and stable, but they have the following disadvantages: the degradation rate is easily limited by the concentration of pesticides.

[0005] Most semiconductor materials have photocatalytic properties. Semiconductor photocatalytic technology is highly efficient, mild, long-lasting, and safe, and is widely used in the degradation of pollutants. The present invention is based on this method.

[0006] In recent years, the new energy industry represented by photovoltaics has become one of the industries with the most certain development prospects. Photocatalysts can oxidize and decompose organic pollutants into harmless small molecules under light sources such as sunlight and visible light without changing or losing themselves. They have the advantages of being long-lasting, safe, and non-toxic. Therefore, the design, synthesis, and application of new and efficient materials are of great significance for the degradation of residual TC in nature. Summary of the invention

[0007] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a N-ZnO / Ti3C2 photocatalyst.

[0008] Another object of the present invention is to provide a N-ZnO / Ti3C2 photocatalyst prepared by the above method.

[0009] Another object of the present invention is to provide the use of the above-mentioned N-ZnO / Ti3C2 photocatalyst in the degradation of tetracycline antibiotics.

[0010] The purpose of the present invention is achieved through the following solutions:

[0011] A method for preparing a N-ZnO / Ti3C2 photocatalyst comprises the following steps:

[0012] (1) adding LiF and Ti3AlC2 to a HCl solution in sequence, reacting, separating, and drying the precipitate to obtain Ti3C2 powder;

[0013] (2) mixing the zinc salt solution with the 2-methylimidazole (MIM) solution, separating them, and drying the precipitate to obtain a precursor ZIF-L powder;

[0014] (3) The Ti3C2 powder obtained in step (1) and the ZIF-L powder obtained in step (2) are uniformly mixed and calcined to obtain an N-ZnO / Ti3C2 photocatalyst.

[0015] The concentration of the HCl solution in step (1) is 8-10 mol·L -1 .

[0016] The dosage ratio of the HCl solution to LiF in step (1) is 20 mL: 1 g; the mass ratio of LiF to Ti3AlC2 is 1:1.

[0017] The reaction temperature of step (1) is 35-40°C and the reaction time is 48h.

[0018] The separation in step (1) is performed by centrifugation at a speed of 4000-4500 rpm for 20 min.

[0019] After the separation in step (1), 2-4 mol·L -1 The precipitate was washed 3 times with HCl solution.

[0020] The drying obtained in step (1) is freeze-drying.

[0021] The zinc salt in step (2) is zinc nitrate.

[0022] The molar ratio of the zinc salt to 2-methylimidazole in step (2) is 1:8.

[0023] The drying in step (2) is vacuum drying at a temperature of 50-60°C.

[0024] The molar ratio of Ti3C2 to ZIF-L in step (3) is 0.4-0.5:1

[0025] The uniform mixing in step (3) specifically comprises firstly dissolving the two powders in water respectively, ultrasonically treating, separating, and drying the precipitate.

[0026] The calcination temperature in step (3) is 400° C. and the calcination time is 2 h.

[0027] The heating rate of the calcination in step (3) is 2°C / min.

[0028] N-ZnO / Ti3C2 photocatalyst prepared by the above method.

[0029] Application of the above-mentioned N-ZnO / Ti3C2 photocatalyst in the degradation of tetracycline antibiotics.

[0030] The mechanism of the present invention is:

[0031] The present invention prepares the precursor ZIF-L of N-ZnO with zinc salt and 2-methylimidazole (MIM), and further calcines the ZIF-L / Ti3C2 composite to prepare the N-ZnO / Ti3C2 photocatalyst by etching Ti3AlC2 to obtain multilayer Ti3C2. The present invention modifies ZnO by doping N and synergizing Ti3C2 composite, thereby improving the photocatalytic performance of ZnO.

[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0033] 1. The present invention dopes N into ZnO: N doping helps ZnO to transform from an n-type semiconductor structure to a p-type semiconductor structure, resulting in a narrower energy band of ZnO and a smaller band gap of ZnO, thereby increasing the separation efficiency of photogenerated carriers and improving the photocatalytic efficiency of ZnO.

[0034] 2. The present invention composites Ti3C2 in N-ZnO: Ti3C2 can be used as a highly efficient synergistic catalyst of N-ZnO, and is more conducive to the migration of photogenerated carriers, thereby improving the photocatalytic efficiency of the material.

[0035] 3. The present invention combines 2D ZIF-L nanosheets and 2D Ti3C2: 2D ZIF-L nanosheets, a precursor of N-ZnO, and 2D Ti3C2 are combined together to obtain a ZIF-L / Ti3C2 composite material, which is further calcined to prepare an N-ZnO / Ti3C2 photocatalyst, providing a new possibility for the preparation of MOF-derived semiconductor / Ti3C2 photocatalysts.

[0036] 4. The N-ZnO / Ti3C2 catalyst obtained by the present invention has excellent adsorption performance and photocatalytic degradation performance for tetracycline antibiotics. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 XRD spectra of Ti3AlC2 and Ti3C2.

[0038] Figure 2 XRD spectra of ZnO, Ti3C2, N-ZnO and N-ZnO / Ti3C2.

[0039] Figure 3 SEM images of Ti3AlC2 (a), Ti3C2 (b), ZIF-L (c), ZnO (d), N-ZnO (e) and N-ZnO / Ti3C2 (f).

[0040] Figure 4 XPS spectra of all elements (a), C 1s (b), N 1s (c), O 1s (d), Ti 2p (e), and Zn 2p (f) of N-ZnO / Ti3C2.

[0041] Figure 5 This is the adsorption curve of TC on N-ZnO / Ti3C2.

[0042] Figure 6 This is the pseudo-first-order kinetic model for the adsorption of TC on N-ZnO / Ti3C2.

[0043] Figure 7 This is the pseudo-second-order kinetic model for the adsorption of TC on N-ZnO / Ti3C2.

[0044] Figure 8 Kinetic fitting curves of TC degradation by different materials.

[0045] Fig. 9 Comparison of TC degradation rate by N-ZnO / Ti3C2 after capturing different free radicals

[0046] Fig.10 This is the photocatalytic degradation mechanism diagram of TC by N-ZnO / Ti3C2. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0048] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0049] Example

[0050] 1) Synthesis of Ti3C2

[0051] Take 20mL of 9mol·L -1HCl solution was added to a polytetrafluoroethylene beaker, and 1.0 g LiF powder was slowly added to the above solution under stirring, and stirred for 10 min; 1.0 g Ti3AlC2 powder was slowly added in portions and the addition time was controlled within 20 min to avoid overheating; stirring was continued at 35 °C for 48 h; centrifuged at 4000 rpm for 20 min, and 3 mol·L -1 The mixture was washed with HCl solution for 3 times to remove the residual LiF after the reaction, and then washed repeatedly with deionized water until the pH of the supernatant was neutral; the precipitate was completely freeze-dried, and the obtained powder was multilayer Ti3C2 powder.

[0052] 2) Synthesis of ZnO

[0053] Pure ZnO can be obtained by heating 3.0 g Zn(CH3COO)2·2H2O to 600°C at a rate of 5°C / min and maintaining it for 3 h.

[0054] 3) Synthesis of N-ZnO

[0055] Weigh 0.595g Zn(NO3)2·6H2O and 1.313g 2-methylimidazole (MIM) and dissolve them in 40ml distilled water respectively. Quickly mix the above Zn(NO3)2 solution and MIM solution. Slowly stir the mixed solution for 4h. Centrifuge. Wash the obtained white precipitate with distilled water and centrifuge for 3 times. Dry it at 60℃ in vacuum overnight. Get ZIF-L precursor. Heat ZIF-L to 400℃ at 2℃ / min. After calcining at 400℃ for 2h, the brown product obtained is N-ZnO.

[0056] 4) Synthesis of N-ZnO / Ti3C2

[0057] 1.0 g (0.0026 mol) of ZIF-L precursor and 0.20 g (0.0011 mol) of Ti3C2 powder were dissolved in 20 mL of distilled water respectively. The two were mixed evenly and stirred for 1 hour, and then ultrasonically treated for 1 hour. The obtained precursor solution was centrifuged and washed with distilled water 3 times, and vacuum dried overnight; the mixture was then transferred to a muffle furnace, the temperature was increased to 400°C at a rate of 2°C / min, and then maintained for 2 hours; after cooling to room temperature, the sample was taken out of the crucible to obtain a N-ZnO / Ti3C2 composite material.

[0058] Test Example:

[0059] 1) Adsorption experiment

[0060] Place 50mL of 20mg / L TC solution in a beaker, add 40mg of N-ZnO / Ti3C2 powder to the solution, and stir to mix evenly. Stir the mixture in a dark place, take an appropriate amount of the mixture every 10 minutes, filter the solution with a 0.45μm filter head, measure its absorbance at 356nm with a UV-visible spectrophotometer, and calculate the corresponding TC concentration.

[0061] 2) Photocatalytic degradation experiment

[0062] Place 50mL of 20mg / L TC solution in a beaker, add 40mg of N-ZnO / Ti3C2 powder to the solution, and stir to mix evenly. Stir the mixture for 40min in a dark place, then place it under a xenon light source, take an appropriate amount of the solution every 20min, filter the solution with a 0.45μm filter, and measure its absorbance at 356nm using a UV-visible spectrophotometer to calculate the corresponding TC concentration.

[0063] 3) Experiment on the photocatalytic degradation mechanism of the system

[0064] 50mL of 20mg / L TC solution was stirred in the dark for 40min, and then 0.001mol / L p-benzoquinone (BQ), disodium ethylenediaminetetraacetate (EDTA-2Na), and isopropyl alcohol (IPA) solutions were added to the solution respectively. The solution was irradiated with a xenon lamp, and an appropriate amount of the above solution was taken every 20min. The solution was filtered with a 0.45μm filter head and its absorbance was measured at 356nm by a UV-visible spectrophotometer to calculate the corresponding TC concentration.

[0065] Results and analysis:

[0066] (1) In order to prove the successful preparation of N-ZnO / Ti3C2 materials, X-ray diffraction (XRD) was performed on Ti3AlC2, Ti3C2, ZnO, N-ZnO and N-ZnO / Ti3C2 materials to analyze the crystal structure and phase composition of the samples. XRD used CuKɑ radiation with a wavelength of 154 pm and a scanning range of 2θ = 20-80°.

[0067] Figure 1 The XRD diffraction patterns of Ti3AlC2 and Ti3C2 are shown. The diffraction peaks of the MXene sample at 33.9°, 39°, 41.7°, and 60.2° correspond to the typical Ti3C2Tx crystal planes (101), (104), (105), and (110), respectively. Compared with the raw material Ti3AlC2, the strongest diffraction peak of the (104) crystal plane near 2θ=39° disappears, indicating that the aluminum atomic layer of Ti3AlC2 was successfully etched by HF, indicating that Ti3AlC2 was completely converted into Ti3C2.

[0068] Figure 2 The peaks of ZIF-L derived N-ZnO at 36.3°, 34.5° and 31.8° are attributed to the (101), (002) and (100) diffraction planes of ZnO, respectively. The crystal planes of N-ZnO can be observed in the composite material N-ZnO / Ti3C2, however, the characteristic peaks of Ti3C2 are almost invisible in the nanocomposite, which may be due to the smaller diffraction peak intensity of Ti3C2 and the lower composite amount of Ti3C2.

[0069] Depend on Figure 3 As shown in a, Ti3AlC2 presents a block-like stacking structure when it is not etched; Figure 3 Figure b shows that after etching Ti3AlC2 with lithium fluoride / hydrochloric acid system, the multilayer Ti3C2 material has interlayer gaps, which is a typical MXene two-dimensional layered structure. At the same time, the multilayer Ti3C2 is stacked together to form an accordion-shaped structure. Figure 3 As can be seen in c, the N-ZnO precursor ZIF-L presents a two-dimensional elliptical leaf shape; Figure 3 As shown in (d), monomer ZnO mainly presents a rod-like structure; Figure 3 It can be seen from the figure that the N-doped ZnO material N-ZnO is a layered structure, but it is sintered together, which may be due to the low morphological stability of ZIF-L; Figure 3 Figure f is the morphology of the composite material. A large coupling interface is formed between N-ZnO and Ti3C2. At the same time, part of N-ZnO is loaded on the Ti3C2 thin layer, but some structures of N-ZnO are still in aggregated form, which may be caused by the uneven mixing of ZIF-L and Ti3C2 during preparation.

[0070] (2) The chemical composition and chemical state of N-ZnO / Ti3C2 composite materials were characterized by XPS. Figure 4 Shown:

[0071] Figure 4 Figure a is the full XPS spectrum of the N-ZnO / Ti3C2 composite material. It can be seen that the composite material is mainly composed of C, N, O, Ti, and Zn elements. Figure 4 b is the XPS spectrum of C1s, and it can be clearly seen that the element has three different characteristic peaks at 284.8eV, 285.8eV and 288.2eV, which are respectively attributed to the CC bond of Ti3C2 in the composite material, the Zn-OC and NC=N bonds of the composite material; Figure 4The spectrum of N1s is shown in Figure c. The characteristic peak at 399.3 eV is caused by the N-Zn-O bond in N-ZnO, indicating the effective synthesis of N-ZnO. The characteristic peak at 398.6 eV belongs to the CN=C bond. Figure 4 Figure d is the XPS spectrum of O1s, which shows two sub-peaks at 531.7 eV and 530.4 eV, matching the Zn-OC bond and Zn-O bond, respectively; Figure 4 Figure e shows the spectrum of Ti 2p, where 461.1eV and 455.0eV are peaks associated with Ti-C bonds and 464.0eV and 458.7eV are peaks corresponding to Ti-O bonds. The peak attributable to Ti-C is weak because the doping amount of Ti3C2 is low; Figure 4 In the figure, f is the XPS spectrum of Zn 2p. Two peaks appear at 1022.5 eV and 1045.1 eV for Zn 2p3 / 2 and Zn 2p1 / 2, respectively, which is related to the presence of ZnO in the composite material.

[0072] In summary, the XPS spectrum shows that the N-ZnO / Ti3C2 composite material was successfully prepared.

[0073] (3) Evaluation of adsorption performance of composite material N-ZnO / Ti3C2:

[0074]

[0075] q t : adsorption capacity of adsorbent on the substance to be adsorbed, unit: mg / g; C0: original concentration of the substance to be adsorbed, unit: mg / L; C t : The concentration of the substance to be adsorbed at time t, unit: mg / L; m: The mass of the catalyst, unit: g; V: The volume of the solution of the substance to be adsorbed, unit: L.

[0076] The adsorption curve of TC on N-ZnO / Ti3C2 is shown in Figure 5 When m = 40 mg, C0 = 20 mg / L, the adsorption of TC by N-ZnO / Ti3C2 increases rapidly within 0-20 min, and basically reaches the adsorption-desorption equilibrium after 40 min. The equilibrium adsorption capacity (q e ) is 12.216 mg / g, and the adsorption rate is 47.71%. Therefore, 40 min can be selected as the dark reaction time to investigate the photocatalytic degradation performance of the composite material on TC.

[0077] (4) The adsorption effect of the composite material N-ZnO / Ti3C2 on TC was detected by analyzing the adsorption kinetics. The adsorption kinetics was described by the Lagergren model of the Langmuir adsorption isotherm equation:

[0078] Pseudo-first-order kinetic model:

[0079] Pseudo-second-order kinetic model:

[0080] Depend on Figure 6 , Figure 7 It can be seen that the correlation coefficients of the pseudo-first-order and pseudo-second-order kinetic equations are R 2 =0.9085 and R 2 =0.9431, indicating that the adsorption of TC by the composite material N-ZnO / Ti3C2 is more consistent with the second-order reaction kinetic model, which shows that the adsorption of TC by the composite material is mainly chemical adsorption. The equilibrium adsorption amount q e =15.97 mg / g, adsorption rate constant k = 0.00493 g / (mg·min).

[0081] (5) Photocatalytic degradation performance of N-ZnO / Ti3C2:

[0082]

[0083] R: The degradation rate of the target pollutant by the catalyst, unit: %; C0: The original concentration of the target degradation substance, unit: mg / L; C t : The concentration of the target degradation substance at time t, unit: mg / L.

[0084] Photocatalytic degradation curves of different materials Figure 8 As shown. When the catalyst dosage is 40 mg and C0 = 20 mg / L, TC is relatively stable and not easy to be photolyzed. Therefore, when no catalyst is added, TC is almost not degraded under xenon lamp irradiation. At the same time, Ti3C2, as a co-catalyst, has poor photocatalytic performance itself, so it cannot photocatalytically degrade TC alone. After 180 minutes of illumination, the photocatalytic degradation rates of TC by ZnO, N-ZnO, and N-ZnO / Ti3C2 were 58.54%, 77.91%, and 86.57%, respectively. It can be seen that compared with ZnO, the degradation rate of TC by ZnO doped with N and composited with Ti3C2 is improved to a certain extent. And the degradation rate of TC by the composite material N-ZnO / Ti3C2 within 180 minutes is 1.48 times that of the monomer ZnO, which greatly improves the photocatalytic degradation efficiency of TC by the photocatalyst, indicating that the doping of N in ZnO and the composite of Ti3C2 have a synergistic effect and have better photocatalytic ability.

[0085] (6) Kinetic analysis of N-ZnO / Ti3C2 photocatalytic degradation reaction:

[0086] The first-order reaction kinetic expression of photocatalytic degradation is: ln(C0 / C t )=kt Formula (5)

[0087] C0: original concentration of target degradation substance, unit: mg / L; C t : The concentration of the target degradation substance at time t, unit: mg / L; k: The first-order reaction rate constant of the photocatalytic degradation process, unit: min -1 ; t: photocatalytic degradation reaction time, unit: min.

[0088] The results are as follows Figure 8 As shown. The photocatalytic degradation of TC by the composite material N-ZnO / Ti3C2 conforms to the first-order reaction kinetic model, and the relevant parameters are shown in Table 1. The apparent rate constants k of N-ZnO and N-ZnO / Ti3C2 are 1.14 and 2.19 times that of monomer ZnO, respectively. This shows that doping N and composite Ti3C2 are beneficial to improving the photocatalytic degradation activity of ZnO.

[0089] Table 1 Kinetic parameters of various materials

[0090]

[0091] (7) Analysis of photocatalytic degradation mechanism of N-ZnO / Ti3C2

[0092] In the exploration of active species, BQ, EDTA-2Na and IPA were used as O2-, h + The degradation mechanism of the photocatalytic reaction system was investigated by scavenging agents of ·OH and ·OH. Fig. 9 As shown in Figure 2. Without adding free radical scavengers, the degradation rate of TC by N-ZnO / Ti3C2 was 86.57%. After adding ·OH and ·O2- scavengers, the degradation rates dropped to 76.87% and 60.40%, respectively. + When the capture agent was added, the degradation rate dropped to 37.68%. It can be seen that after capturing ·OH and ·O2-, the photocatalytic efficiency of the composite material N-ZnO / Ti3C2 for TC was inhibited to a certain extent, while the capture of h + After that, the photocatalytic efficiency of TC degradation of this material was inhibited to the maximum, which can be explained that the active species h in this photocatalytic degradation system + The greatest impact on TC degradation is O2 - , and finally OH, which can be explained by h + The active substances that play a major role in the photocatalytic degradation of TC by the composite material are ·OH and ·O2 - It also played a partial role.

[0093] The above mechanism analysis results show that the photocatalytic degradation mechanism of TC by the composite material N-ZnO / Ti3C2 can be explained as follows: under light, the electrons on the VB of ZnO in the composite material N-ZnO / Ti3C2 absorb the corresponding energy and are excited and transition to the CB, generating photogenerated electron-hole pairs (e - -h + ). Doping N into ZnO changes the structure of ZnO from an n-type semiconductor to a p-type semiconductor, resulting in a decrease in the band gap energy of VB and a large amount of h + The generation of ZnO narrows the energy band and reduces the band gap of ZnO, thereby increasing the separation efficiency of photogenerated carriers. At the same time, Ti3C2 can be used as an efficient synergistic catalyst of N-ZnO, and the two form a relatively close interface contact, e - Transfer from N-ZnO CB to Ti3C2 layer, h + It remains on the valence band of N-ZnO, e - and h + The separation probability of photogenerated charge carriers is greatly improved, which is more conducive to the migration of photogenerated charge carriers. - and h + It can react with oxygen on the catalyst surface or water in the solution to produce active groups with strong oxidizing properties, OH, and active groups with strong reducing properties, O2. - Both types of active groups can react with pollutants. + It is also an active substance with strong oxidizing effect, which can directly oxidize and degrade pollutants, thereby achieving the purpose of degrading organic pollutants.

[0094] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A N-ZnO / Ti 3 C 2 A method for preparing a photocatalyst, It is characterized in that The following steps are involved: (1) LiF and Ti were added to the HCl solution in sequence. 3 AlC 2 , react, separate, and dry the precipitate to obtain Ti 3 C 2 powder; (2) mixing the zinc salt solution and the 2-methylimidazole solution, separating them, and drying the precipitate to obtain a precursor ZIF-L powder; (3) Ti obtained in step (1) 3 C 2 The powder is mixed evenly with the ZIF-L powder obtained in step (2), and calcined to obtain N-ZnO / Ti 3 C 2 Photocatalyst.

2. N-ZnO / Ti according to claim 1 3 C 2 Method for preparing photocatalyst, Features: The concentration of the HCl solution in step (1) is 8-10 mol·L -1 .

3. N-ZnO / Ti according to claim 1 3 C 2 Method for preparing photocatalyst, Features: The ratio of HCl solution to LiF in step (1) is 20 mL:1 g; LiF to Ti 3 AlC 2 The mass ratio is 1:

1.

4. N-ZnO / Ti according to claim 1 3 C 2 A method for preparing a photocatalyst, Features: The reaction temperature in step (1) is 35-40°C and the reaction time is 48h; After the separation in step (1), 2-4 mol·L -1 The precipitate was washed three times with HCl solution; The drying obtained in step (1) is freeze-drying.

5. N-ZnO / Ti according to claim 1 3 C 2 Method for preparing photocatalyst, Features: The zinc salt in step (2) is zinc nitrate; The molar ratio of the zinc salt to 2-methylimidazole in step (2) is 1:

8.

6. N-ZnO / Ti according to claim 1 3 C 2 A method for preparing a photocatalyst, Features: The drying in step (2) is vacuum drying at a temperature of 50-60°C.

7. N-ZnO / Ti according to claim 1 3 C 2 Method for preparing photocatalyst, Features: Step (3) Ti 3 C 2 The molar ratio with ZIF-L is 0.4-0.5:1; The uniform mixing in step (3) specifically comprises firstly dissolving the two powders in water respectively, ultrasonically treating, separating, and drying the precipitate.

8. The N-ZnO / Ti according to claim 1 3 C 2 A method for preparing a photocatalyst, Features: The calcination temperature in step (3) is 400° C. and the calcination time is 2 h. The heating rate of the calcination in step (3) is 2°C / min.

9. N-ZnO / Ti prepared by the method according to any one of claims 1 to 8 3 C 2 Photocatalyst.

10. N-ZnO / Ti as claimed in claim 9 3 C 2 Application of photocatalysts in the degradation of tetracycline antibiotics.