Ionic liquid functionalized magnetic nanoparticles as well as preparation method and application thereof

By functionalizing magnetic nanoparticle catalysts with ionic liquids and loading ionic liquids under mild conditions using a stepwise grafting method, the problem of high temperature and high pressure in PET recycling was solved, achieving efficient and safe PET degradation, which is suitable for large-scale production.

CN118925799APending Publication Date: 2024-11-12ZHEJIANG LANDE ENERGY TECHNOLOGY DEVELOPMENT CO LTD

Patent Information

Application Number
CN202410982786.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Among existing PET recycling methods, mechanical recycling has poor quality and cannot completely recycle PET, while chemical recycling requires high temperature and high pressure, which is costly and inefficient. Furthermore, traditional catalysts are unsafe during acid treatment, and magnetic nanoparticles are easily decomposed and difficult to control.

Method used

Magnetic nanoparticles functionalized with ionic liquids were used as catalysts. Ionic liquids were loaded onto the surface of the magnetic nanoparticles through a stepwise grafting method, avoiding the use of strong acids. A silica layer was used to protect the grafting process from the introduction of water, thereby improving the ionic liquid loading efficiency. Mild reaction conditions were also employed.

Benefits of technology

It achieves efficient and safe PET degradation, improves the yield and rate of PET degradation to BHET, is suitable for large-scale production, reduces energy consumption and costs, and improves the resource utilization efficiency of waste PET.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956558270000061
    Figure BDA0004956558270000061
Patent Text Reader

Abstract

The invention belongs to the technical field of catalytic chemistry, and provides ionic liquid functionalized magnetic nanoparticles as well as a preparation method and application thereof. The method comprises the following steps: (1) mixing a Fe3O4 nano-particle solution and tetraethyl silicate for reaction to obtain a magnetic nano-particle precursor; (2) under a protective atmosphere, mixing the magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and a solvent, and carrying out a reaction to obtain a magnetic nanoparticle intermediate; and (3) mixing the magnetic nanoparticle intermediate, N-methylimidazole and a solvent for reaction to obtain the ionic liquid functionalized magnetic nanoparticles. According to the method, the ionic liquid functionalized magnetic nanoparticles are used as a catalyst, a silicon dioxide layer is activated at high temperature in the process of grafting the ionic liquid, silanol and the ionic liquid are grafted step by step, and efficient degradation of PET is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalytic chemistry, and in particular to an ionic liquid functionalized magnetic nanoparticle and a preparation method and application thereof. Background Art

[0002] Polyethylene terephthalate (PET) is a plastic material widely used in packaging, textiles and other fields. However, with the improvement of environmental awareness, how to effectively recycle and reuse waste PET has become an important research topic. At present, the main recycling methods of PET include mechanical recycling and chemical recycling. Mechanical recycling mainly reprocesses waste PET into new plastic products through crushing, cleaning, drying and other steps, but the quality of recycled PET obtained by this method is poor, and it is impossible to achieve complete recycling of waste PET. Chemical recycling decomposes PET into monomers or oligomers through chemical reactions, and then further synthesizes new PET or other useful chemicals. This method can achieve complete recycling of waste PET, but the current chemical recycling method often requires harsh conditions such as high temperature and high pressure, high energy consumption, high cost, and low efficiency. When the new PET degradation catalyst is used for recycling, acid is used for activation treatment in the catalyst synthesis path. High concentration of acid is extremely unsafe in large-scale chemical production, and magnetic nanoparticles are easily decomposed during the acid treatment process, and the experimental progress is difficult to control. Therefore, a new, efficient and low-cost PET degradation and recycling method is of great significance for the resource utilization of waste PET. Summary of the invention

[0003] The purpose of the present invention is to overcome the defects in the prior art and provide an ionic liquid functionalized magnetic nanoparticle and a preparation method and application thereof.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing ionic liquid functionalized magnetic nanoparticles, comprising the following steps:

[0006] (1) mixing a Fe3O4 nanoparticle solution and tetraethyl silicate to react to obtain a magnetic nanoparticle precursor;

[0007] (2) under a protective atmosphere, mixing a magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and a solvent to react to obtain a magnetic nanoparticle intermediate;

[0008] (3) Mixing the magnetic nanoparticle intermediate, N-methylimidazole and a solvent for reaction to obtain the ionic liquid functionalized magnetic nanoparticles.

[0009] Preferably, the Fe3O4 nanoparticle solution in step (1) comprises Fe3O4 nanoparticles, ethanol and ammonia water;

[0010] The mass volume ratio of the Fe3O4 nanoparticles, ethanol and ammonia water is 4-6 g: 80-120 mL: 10-20 mL;

[0011] The mass fraction of the ammonia water is 20-30%.

[0012] Preferably, the mass volume ratio of the Fe3O4 nanoparticles to tetraethyl silicate is 4-6 g:3-5 mL.

[0013] Preferably, the reaction temperature in step (1) is 25-35° C. and the reaction time is 4-8 h.

[0014] Preferably, the solvent in step (2) is toluene and / or xylene;

[0015] The mass ratio of the magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and solvent in step (2) is 1:0.05-0.8:5-20.

[0016] Preferably, the reaction temperature in step (2) is 40-60° C. and the reaction time is 4-8 h.

[0017] Preferably, the solvent in step (3) is toluene and / or xylene;

[0018] The mass ratio of the magnetic nanoparticle intermediate, N-methylimidazole and solvent in step (3) is 1:0.02 to 2:5 to 20.

[0019] Preferably, the reaction temperature in step (3) is 80-120° C. and the reaction time is 10-14 h.

[0020] The present invention also provides the ionic liquid functionalized magnetic nanoparticles prepared by the preparation method of the ionic liquid functionalized magnetic nanoparticles.

[0021] The invention also provides application of the ionic liquid functionalized magnetic nanoparticles in degrading polyethylene terephthalate.

[0022] The present invention provides a method for preparing ionic liquid functionalized magnetic nanoparticles, comprising the following steps: (1) mixing a Fe3O4 nanoparticle solution and tetraethyl silicate to react, thereby obtaining a magnetic nanoparticle precursor; (2) mixing the magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and a solvent to react, thereby obtaining a magnetic nanoparticle intermediate under a protective atmosphere; (3) mixing the magnetic nanoparticle intermediate, N-methylimidazole and a solvent to react, thereby obtaining the ionic liquid functionalized magnetic nanoparticles. The present invention uses ionic liquid functionalized magnetic nanoparticles as catalysts, activates a silicon dioxide layer at high temperature during the grafting of ionic liquids, and grafts silanol and ionic liquids in steps. Benzene organic solvents such as xylene and toluene are used to protect the silicon dioxide layer from water introduction during the grafting process, thereby allowing more ionic liquids to be grafted onto the surface of the magnetic nanoparticles, which is beneficial for efficient degradation of PET.

[0023] The preparation method provided by the present invention has a mild synthesis process: the present invention adopts a step-by-step grafting method to load the ionic liquid, no strong acid is added during the process, and the reaction is safe and controllable. High loading efficiency: the synthesis method of the present invention can effectively improve the efficiency of ionic liquid loading on magnetic nanoparticles, shorten the production time, save energy, and meet the needs of large-scale production. High degradation efficiency: the catalyst of the present invention can effectively promote the degradation of PET, improve the yield of the process of PET degradation to BHET, increase the degradation rate, shorten the degradation time, and realize the batch recovery and degradation of waste PET, which is suitable for large-scale production. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing ionic liquid functionalized magnetic nanoparticles, comprising the following steps:

[0025] (1) mixing a Fe3O4 nanoparticle solution and tetraethyl silicate to react to obtain a magnetic nanoparticle precursor;

[0026] (2) under a protective atmosphere, mixing a magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and a solvent to react to obtain a magnetic nanoparticle intermediate;

[0027] (3) Mixing the magnetic nanoparticle intermediate, N-methylimidazole and a solvent for reaction to obtain the ionic liquid functionalized magnetic nanoparticles.

[0028] In the present invention, the Fe3O4 nanoparticle solution in step (1) comprises Fe3O4 nanoparticles, ethanol and ammonia water.

[0029] In the present invention, the mass volume ratio of the Fe3O4 nanoparticles, ethanol and ammonia water is preferably 4-6 g: 80-120 mL: 10-20 mL, more preferably 4.5-5.5 g: 85-115 mL: 12-18 mL, and more preferably 4.8-5.2 g: 90-110 mL: 14-16 mL.

[0030] In the present invention, the mass fraction of the aqueous ammonia is preferably 20 to 30%, more preferably 22 to 28%, and even more preferably 24 to 26%.

[0031] In the present invention, Fe3O4 nanoparticles, ethanol and ammonia water are mixed and stirred, and the stirring temperature is preferably 25-35°C, more preferably 26-34°C, and more preferably 28-32°C; the stirring time is preferably 10-20 min, more preferably 12-18 min, and more preferably 14-16 min.

[0032] In the present invention, the mass volume ratio of the Fe3O4 nanoparticles and tetraethyl silicate is preferably 4-6 g: 3-5 mL, more preferably 4.5-5.5 g: 3.5-4.5 mL, and more preferably 4.8-5.2 g: 3.8-4.2 mL.

[0033] In the present invention, the reaction temperature in step (1) is preferably 25-35°C, more preferably 26-34°C, more preferably 28-32°C; the reaction time is preferably 4-8h, more preferably 4.5-7.5h, more preferably 5-6h; the stirring speed is preferably 300-400rpm, more preferably 320-380rpm, more preferably 340-360rpm; the reaction in step (1) is carried out in a protective atmosphere, and the protective atmosphere is preferably nitrogen, helium or neon.

[0034] In the present invention, after the reaction in step (1) is completed, the solid is recovered by a magnet, and then the solid is washed with ethanol and then dried; the drying temperature is preferably 40-50°C, more preferably 42-48°C, and more preferably 44-46°C; the time is preferably ≥12h, more preferably ≥14h, and more preferably ≥16h; after drying, a magnetic nanoparticle precursor is obtained.

[0035] In the present invention, the reaction mechanism of step (1) is as follows: In the process of preparing silica microspheres by the Stober method, the addition of ammonia water makes the ferroferric oxide nanoparticles electronegative. This is because the divalent iron in the ferroferric oxide nanoparticles easily loses electrons and is oxidized, and its surface easily adsorbs hydroxide ions, making the ferroferric oxide nanoparticles electronegative. After tetraethyl silicate is added to the solvent, the ammonium ions on the surface of the microspheres adsorb the negatively charged silicon alkoxide precursor SiO -In this way, the ammonium ions can serve as a bridge between the ferroferric oxide nanoparticles and the silicon alkoxide precursor groups. When the silicon alkoxide precursor is adsorbed onto the surface of ferroferric oxide, it will hydrolyze to form a uniform and stable coating shell.

[0036] In the present invention, the solvent in step (2) is preferably toluene and / or xylene.

[0037] In the present invention, the mass ratio of the magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and solvent in step (2) is preferably 1:0.05-0.8:5-20, more preferably 1:0.1-0.7:8-17, and more preferably 1:0.2-0.6:10-15.

[0038] In the present invention, the protective atmosphere in step (2) is preferably nitrogen, helium or neon.

[0039] In the present invention, the reaction temperature in step (2) is preferably 40-60°C, more preferably 45-55°C, more preferably 48-52°C; the reaction time is preferably 4-8h, more preferably 5-7h, more preferably 5.5-6.5h.

[0040] In the present invention, after the reaction in step (2) is completed, the solid is naturally cooled to room temperature, and the solid is recovered by a magnet, and washed with toluene and ethanol in sequence; the number of toluene washings is preferably ≥2 times, more preferably ≥3 times, and more preferably ≥4 times; the number of ethanol washings is preferably ≥2 times, more preferably ≥3 times, and more preferably ≥4 times; after washing, drying is performed, and the drying temperature is preferably 50-70°C, more preferably 55-65°C, and more preferably 58-62°C; the drying time is preferably ≥4h, more preferably ≥5h, and more preferably ≥6h; after drying, the magnetic nanoparticle intermediate is obtained.

[0041] In the present invention, the reaction mechanism of step (2) is as follows: the silanol shell generated in step (1) reacts with the methoxysilyl group in the added 3-chloropropyltrimethoxysilane, and methanol is removed during the whole process, so that the silanol and the silicon in the 3-chloropropyltrimethoxysilane are connected to the same oxygen atom in the form of a covalent bond.

[0042] In the present invention, the solvent in step (3) is preferably toluene and / or xylene.

[0043] In the present invention, the mass ratio of the magnetic nanoparticle intermediate, N-methylimidazole and solvent in step (3) is preferably 1:0.02-2:5-20, more preferably 1:0.5-1.5:10-15, and more preferably 1:0.8-1.2:12-13.

[0044] In the present invention, the reaction temperature in step (3) is preferably 80-120°C, more preferably 85-115°C, more preferably 90-110°C; the reaction time is preferably 10-14h, more preferably 11-13h, more preferably 11.5-12.5h.

[0045] In the present invention, after the reaction in step (3) is completed, the solid is filtered to obtain a solid, and then washed with toluene and ethanol in sequence; the number of washings with toluene is preferably ≥3 times, more preferably ≥4 times, and more preferably ≥5 times; the number of washings with ethanol is preferably ≥3 times, more preferably ≥4 times, and more preferably ≥5 times; after the washing, the solid is dried, and the drying temperature is preferably 70 to 90° C., more preferably 75 to 85° C., and more preferably 77 to 83° C.; and the ionic liquid functionalized magnetic nanoparticles are obtained by drying to a constant weight.

[0046] In the present invention, the reaction mechanism of step (3) is as follows: 3-chloropropyltrimethoxysilane undergoes an electrophilic addition reaction with N-methylimidazole. The chlorine in 3-chloropropyltrimethoxysilane has a strong electron-withdrawing ability. After N-methylimidazole is added to the solvent, the chlorine atom will attack the carbon-nitrogen double bond with a larger electron cloud density on N-methylimidazole and form a bond with it. The π bond in the carbon-nitrogen double bond breaks and forms two new σ bonds with 3-chloropropyltrimethoxysilane. The chlorine atom induces the electron cloud to migrate toward it and is electronegative, while the nitrogen atom is positively charged.

[0047] The present invention also provides ionic liquid functionalized magnetic nanoparticles prepared by the preparation method of the ionic liquid functionalized magnetic nanoparticles.

[0048] The present invention also provides application of the ionic liquid functionalized magnetic nanoparticles in degrading polyethylene terephthalate.

[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0050] Example 1

[0051] Mix 5 g of Fe3O4 nanoparticles, 100 mL of ethanol and 15 mL of ammonia water (25%), stir at 30°C for 15 min, then add 4 mL of tetraethyl silicate, and react at 360 rpm for 6 h in a nitrogen atmosphere at 30°C. After the reaction, recover the solid with a magnet, wash with ethanol and dry at 45°C for 12 h to obtain a magnetic nanoparticle precursor.

[0052] Mix 3 g of magnetic nanoparticle precursor, 0.6 g of 3-chloropropyltrimethoxysilane and 15 g of toluene, and react under a nitrogen atmosphere at 50 °C for 6 h. After the reaction is completed, naturally cool to room temperature, recover the solid with a magnet, wash twice with toluene, wash twice with ethanol, and then dry at 60 °C for 4 h to obtain a magnetic nanoparticle intermediate.

[0053] 3 g of magnetic nanoparticle intermediate, 5 g of N-methylimidazole and 15 g of toluene were mixed, refluxed at 100° C. for 12 h, and the solid was filtered out. The solid was washed with toluene 3 times, ethanol 3 times, and then dried at 80° C. to constant weight to obtain ionic liquid functionalized magnetic nanoparticles.

[0054] Degradation effect test:

[0055] PET film: 5 g, ionic liquid functionalized magnetic nanoparticles: 0.75 g, ethylene glycol: 50 mL, betaine salicylate: 0.15 g, activated carbon: 2 g.

[0056] Ionic liquid functionalized magnetic nanoparticles were used as catalysts, ethylene glycol was used as solvent, betaine was added, and PET film was added at the same time, and the reaction was carried out at 190°C for 6 hours. It was observed that there was still some unreacted at the bottom of the flask, and stirring was continued until the reaction was complete, and the reaction lasted for 12 hours. After magnetic separation of the PET degradation mixture, 100 mL of deionized water was added, activated carbon was added, and the mixture was kept at 90°C for 1.5 hours, then cooled to 60°C, stirred and kept warm for 3 hours, and the impurities such as dimers precipitated were filtered, and then placed in a -10°C refrigerator for 24 hours, and the precipitated crystals were filtered and vacuum dried at 60°C. A total of 5.95 g of BHET was collected, and the yield was calculated according to the following formula to obtain a high yield (90%) of the product;

[0057]

[0058] Where:

[0059] W BHET is the mass of BHET solid;

[0060] W PET The quality of PET;

[0061] M BHET is the molar mass of BHET;

[0062] M PET is the molar mass of the repeating structural unit of PET.

[0063] Example 2

[0064] Mix 5 g of Fe3O4 nanoparticles, 100 mL of ethanol and 15 mL of ammonia water (25%), stir at 30°C for 15 min, then add 4 mL of tetraethyl silicate, and react at 340 rpm for 6 h in a nitrogen atmosphere at 30°C. After the reaction, recover the solid with a magnet, wash with ethanol and dry at 45°C for 12 h to obtain a magnetic nanoparticle precursor.

[0065] Mix 3 g of magnetic nanoparticle precursor, 0.24 g of 3-chloropropyltrimethoxysilane and 15 g of toluene, and react under a nitrogen atmosphere at 50 °C for 6 h. After the reaction is completed, naturally cool to room temperature, recover the solid with a magnet, wash twice with toluene, wash twice with ethanol, and then dry at 60 °C for 4 h to obtain a magnetic nanoparticle intermediate.

[0066] 3 g of magnetic nanoparticle intermediate, 0.1 g of N-methylimidazole and 15 g of toluene were mixed, refluxed at 100° C. for 12 h, and the solid was filtered out. The solid was washed with toluene 3 times, washed with ethanol 3 times, and then dried at 80° C. to constant weight to obtain ionic liquid functionalized magnetic nanoparticles.

[0067] Degradation effect test:

[0068] 100 mesh PET powder: 4.675 g, ionic liquid functionalized magnetic nanoparticles: 0.7 g, ethylene glycol: 50 ml, betaine salicylate: 0.1 g.

[0069] Ionic liquid functionalized magnetic nanoparticles were used as catalysts, ethylene glycol was used as solvent, betaine was added and PET powder was added at the same time, and the mixture was reacted at 195°C in a microwave reactor for 3 hours. After magnetic separation of the PET degradation mixture, 100 mL of deionized water was added, and the mixture was kept at 90°C for 1.5 hours, and the precipitated dimer and the like were filtered out, and then the mixture was cooled to 60°C, stirred and kept warm for 2 hours, and the precipitated dimer and other impurities were filtered out, and then the mixture was placed in a -10°C refrigerator for 24 hours, and the precipitated crystals were filtered out, and vacuum dried at 60°C. A total of 5.267 g of BHET was collected, and a high yield (85%) of the product was obtained according to the formula in Example 1.

[0070] As can be seen from the above examples, the present invention provides a method for preparing ionic liquid functionalized magnetic nanoparticles, which can effectively reduce the safety risks in the catalyst production process and reduce potential safety hazards, which is of great significance for large-scale production and personal safety. Secondly, the catalyst of the present invention is an ionic liquid functionalized magnetic nanoparticle, which has the advantages of high activity, high stability and long life, can effectively improve the degradation efficiency of PET, and has important application value in the field of chemical raw material production.

[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing ionic liquid functionalized magnetic nanoparticles, characterized in that: It includes the following steps: (1) mixing a Fe3O4 nanoparticle solution and tetraethyl silicate to react to obtain a magnetic nanoparticle precursor; (2) under a protective atmosphere, mixing a magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and a solvent to react to obtain a magnetic nanoparticle intermediate; (3) Mixing the magnetic nanoparticle intermediate, N-methylimidazole and a solvent for reaction to obtain the ionic liquid functionalized magnetic nanoparticles.

2. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 1, characterized in that: The Fe3O4 nanoparticle solution in step (1) comprises Fe3O4 nanoparticles, ethanol and ammonia water; The mass volume ratio of the Fe3O4 nanoparticles, ethanol and ammonia water is 4-6 g: 80-120 mL: 10-20 mL; The mass fraction of the ammonia water is 20-30%.

3. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 1 or 2, characterized in that: The mass volume ratio of the Fe3O4 nanoparticles to tetraethyl silicate is 4-6 g:3-5 mL.

4. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 3, characterized in that: The reaction temperature in step (1) is 25-35° C. and the reaction time is 4-8 hours.

5. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 1, 2 or 4, characterized in that: The solvent in step (2) is toluene and / or xylene; The mass ratio of the magnetic nanoparticle precursor, 3-chloropropyltrimethoxysilane and solvent in step (2) is 1:0.05-0.8:5-20.

6. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 5, characterized in that: The reaction temperature in step (2) is 40-60° C. and the reaction time is 4-8 hours.

7. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 1 or 6, characterized in that: The solvent in step (3) is toluene and / or xylene; The mass ratio of the magnetic nanoparticle intermediate, N-methylimidazole and solvent in step (3) is 1:0.02 to 2:5 to 20.

8. The method for preparing ionic liquid functionalized magnetic nanoparticles according to claim 7, characterized in that: The reaction temperature in step (3) is 80-120° C. and the reaction time is 10-14 h. 9 . The ionic liquid functionalized magnetic nanoparticles prepared by the method for preparing ionic liquid functionalized magnetic nanoparticles according to any one of claims 1 to 8 .

10. Use of the ionic liquid functionalized magnetic nanoparticles according to claim 9 in the degradation of polyethylene terephthalate.

Citation Information

Patent Citations

  • Ionic liquid functionalized magnetic nanoparticle and preparation method and application thereof

    CN102641702A

  • Basic ionic liquid modified magnetic nanoparticle catalyst for synthesizing biodiesel and preparation method thereof

    CN103212445A

  • Method for degrading polyethylene glycol terephthalate (PET)

    CN103641678A

  • Method for catalytically synthesizing N, N'-disubstituted urea derivative and imidazole derivative

    CN105439908A

  • Method for preparing diisobutyl phthalate

    CN110330428A

Cited By

  • Process for degrading colored waste PET fabric and recycling BHET

    CN121974799A