Hot-rolled ribbed steel bar coiled screw and production process thereof
By adopting chemical composition formulas with high V and low Si and Mn and specific rolling processes, the problem of high production costs of hot-rolled ribbed steel bars is solved, and performance stability and cost reduction are achieved, and product performance is significantly improved.
Patent Information
- Application Number
- CN202410986392.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Due to the implementation of the new national standard, the metallographic structure inspection standards of hot-rolled ribbed steel bars have increased, resulting in an increase in domestic Si and Mn mining, resulting in an increase in the prices of ferrosilicon and silicon-manganese alloys, and the production costs of enterprises have increased significantly, so it is necessary to develop low-cost Chemical composition combination and process methods to stabilize production.
Using chemical composition formulas of high V and low Si and Mn, and through specific rolling process steps, including multiple rolling and cooling treatments, the hot-rolled ribbed steel coils are made. The specific steps include heating, rough rolling, and medium rolling. , pre-finishing rolling, finishing rolling, water-through cooling and silk-spinning molding, controlling chemical composition and rolling parameters to achieve stable performance and reduced cost.
The performance of hot-rolled ribbed steel coils is achieved stable, reducing alloy costs, refined grains, uniform structure, high overall elongation of maximum force, significantly improving product performance, and bringing economic and social benefits.
Smart Images

Figure CN118926303A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot-rolled ribbed steel bars, in particular to a hot-rolled ribbed steel bar coil and a production process thereof. Background Art
[0002] With the implementation of the new national standard for hot-rolled ribbed steel bars for reinforced concrete in 2018, strict inspection standards for the metallographic structure of hot-rolled ribbed steel bars have been added, which has affected the production process and chemical composition formula. At present, the chemical composition formula commonly used in domestic wire rod coil products is C plus high Si, high Mn basis plus trace V or Nb, Ti trace elements. The production of hot-rolled ribbed steel bars adds a large amount of Si and Mn elements, which also intensifies the large-scale mining of domestic Si and Mn mines. The average grade of Mn ore in my country is only 22%, while the average grade of ore in major Mn resource countries in the world is about 40%. In comparison, the grade of Mn ore in my country is much lower than that of other major Mn ore resource countries. While China mines a large amount of Si and Mn ores, it also needs a large amount of imports, resulting in a sharp rise in the prices of domestic ferrosilicon and silicon-manganese alloys, and a significant increase in the production costs of enterprises. The price of vanadium-nitrogen alloy is relatively stable.
[0003] Therefore, under the premise of ensuring product performance, it is particularly important to develop a chemical composition combination and process method for achieving stable and low-cost production of hot-rolled ribbed steel bar coils. Summary of the invention
[0004] To solve the above problems, the present invention provides a hot-rolled ribbed steel bar coil and a production process thereof, which adopts a high V and low Si, Mn chemical composition formula, effectively achieving stable performance and low-cost production of the hot-rolled ribbed steel bar coil.
[0005] The technical solution adopted by the present invention is:
[0006] A production process for hot-rolled ribbed steel bar coils, comprising the following steps:
[0007] S1. Use a square billet with a chemical composition of C: 0.21-0.25%, Si: 0.20-0.35%, Mn: 1.10-1.35%, P≤0.040%, S≤0.040%, V: 0.020-0.030%, Ceq: 0.41-0.49% as the billet, and heat the billet to 1040-1100°C to ensure the rolling start temperature is 990-1020°C;
[0008] S2, descaling the heated steel billet with high-pressure water and then performing rough rolling to obtain a first round rolled piece, shearing the first round rolled piece at the head and tail, and then performing intermediate rolling to obtain a second round rolled piece, shearing the second round rolled piece at the head and tail, and then performing intermediate rolling again to obtain a third round rolled piece, and performing pre-finish rolling on the third round rolled piece to obtain a fourth round rolled piece;
[0009] S3, water-cooling the fourth round rolled piece to cool the temperature of the fourth round rolled piece to 860-900°C, then shearing the cooled fourth round rolled piece at the head and tail, and then finishing rolling to obtain a hot-rolled coil, then water-cooling the hot-rolled coil to cool the temperature of the hot-rolled coil to 960-1010°C, and spinning the cooled hot-rolled coil into a coil.
[0010] Furthermore, in step S3, the specification range of the hot-rolled coil is φ6 mm to φ12 mm, and the preferred chemical composition ratios of each specification are as follows:
[0011] φ6㎜ specification, C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.05~1.15%, P≤0.040%, S≤0.040%, V: 0.020~0.025%, Ceq: 0.41~0.46%;
[0012] φ8mm—φ10㎜ specifications, C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.15~1.25%, P≤0.040%, S≤0.040%, V: 0.020~0.025%, Ceq: 0.42~0.47%;
[0013] φ12㎜Specifications: C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.20~1.35%, P≤0.040%, S≤0.040%, V: 0.025~0.030%, Ceq: 0.43~0.49%.
[0014] Further, in step S2,
[0015] The rough rolling is carried out by a rough rolling mill consisting of 6 rough rolling mills, and the pass types of the 6 rough rolling mills are box type-box type-box type-round type-elliptical type-round type;
[0016] The first intermediate rolling is carried out by an intermediate rolling mill consisting of 6 intermediate rolling mills, and the hole types of the 6 intermediate rolling mills are elliptical-circular-elliptical-circular-elliptical-circular;
[0017] The second intermediate rolling is carried out by an intermediate rolling mill consisting of two intermediate rolling mills, and the hole types of the two intermediate rolling mills are elliptical-circular respectively.
[0018] Furthermore, in step S2, the rolling speed of the pre-finish rolling is controlled at 10 m / s to 13 m / s.
[0019] Further, in step S2,
[0020] To produce coils with a specification of φ6mm to φ8mm, the pre-finishing rolling is carried out by a pre-finishing rolling mill consisting of 4 pre-finishing rolling mills. The hole types of the 4 pre-finishing rolling mills are elliptical-circular-elliptical-circular in sequence.
[0021] For producing coils with specifications of φ10mm to φ12mm, the pre-finishing rolling is carried out by a pre-finishing rolling mill consisting of two pre-finishing rolling mills, and the hole types of the two pre-finishing rolling mills are elliptical and circular respectively.
[0022] Further, in step S3,
[0023] To produce φ6mm hot-rolled coil, the finishing rolling is carried out by a finishing mill consisting of 10 finishing mills. The hole types of the 10 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular-oval-circular;
[0024] To produce φ8mm hot-rolled coils, the finishing rolling is carried out by a finishing mill consisting of 8 finishing mills. The hole types of the 8 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular;
[0025] To produce φ10mm hot-rolled coils, the finishing rolling is carried out by a finishing mill consisting of 8 finishing mills. The hole types of the 8 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular.
[0026] For producing φ12mm hot-rolled coil, finishing rolling is carried out by a finishing mill consisting of 6 finishing mills, and the hole types of the 6 finishing mills are elliptical-circular-elliptical-circular-elliptical-circular.
[0027] Furthermore, in step S3, water cooling is carried out by a water cooling device, the water pressure of the first water cooling device is 0.60-0.80 MPa, and the water flow rate is 20-40 m3 / h; the water pressure of the second water cooling device is 0.60-0.80 MPa, and the water flow rate is 40-80 m3 / h; the water pressure of the third water cooling device is 0.60-0.80 MPa, and the water flow rate is 40-80 m3 / h; the water pressure of the fourth water cooling device is 0.60-0.80 MPa, and the water flow rate is 20-40 m3 / h, wherein the spinning temperature for producing φ6mm-φ8mm specifications is controlled at 980-1010°C, and the spinning temperature for producing φ10mm-φ12mm specifications is controlled at 960-980°C.
[0028] Further, in step S3, the spinning forming is carried out by a spinning machine, the leading coefficient of the spinning machine is 1.010-1.025, the positive amplitude coefficient of the swing is 0.02, the positive amplitude coefficient of the swing is 0.02, and the swing time is 8 seconds.
[0029] Further, in step S3, the coiled conch after spinning is air-cooled by an air-cooled roller, and the air-cooled roller has 11 sections, with a roller speed of 0.45-0.48 m / s in section 1, 0.48-0.51 m / s in section 2, 0.51-0.54 m / s in section 3, 0.54-0.57 m / s in section 4, 0.57-0.60 m / s in section 5, and 0.60 m / s in section 6. The roller speed is 0.60-0.63m / s; the 7th-section roller speed is 0.63-0.66m / s; the 8th-section roller speed is 0.66-0.70m / s; the 9th-section roller speed is 0.70-0.75m / s; the 10th-section roller speed is 0.70-0.75m / s; the 11th-section roller speed is 0.80-0.85m / s; and there are 15 insulation covers in the air cooling process, and all the insulation covers are opened.
[0030] Based on the same inventive concept, the present application also provides a steel bar coil produced using the above-mentioned hot-rolled ribbed steel bar coil production process.
[0031] The beneficial effects of the present invention are as follows:
[0032] The production process of the hot-rolled ribbed steel bar coil provided by the present invention adopts a high-V and low-Si, Mn chemical composition formula to solve the problem of rising prices of ferrosilicon and silicon-manganese alloys through reasonable design of alloy composition and rolling process structure. The formula can achieve stable performance and low-cost production of the hot-rolled ribbed steel bar coil, greatly reducing the alloy cost, and achieving grain refinement, uniform structure, high maximum force total elongation and improved performance of the hot-rolled ribbed steel bar coil, bringing huge economic and social benefits to the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the system layout used in the production process of the present invention.
[0034] Reference numerals
[0035] Heating furnace 1, high-pressure water descaling device 2, roughing mill unit 3, No. 1 flying shear 4, first intermediate rolling mill unit 5, No. 2 flying shear 6, second intermediate rolling mill unit 7, pre-finishing mill unit 8, pre-water cooling device 9, No. 3 flying shear 10, finishing mill unit 11, water cooling device 12, laying head 13, air-cooled roller table 14, fan 15, insulation cover 16, coil core stand 17, P&F line 18. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively by way of examples, and preferred embodiments of the present invention are given below. However, the present invention can be implemented in a variety of different forms and is not limited to the embodiments described herein. Any other implementation schemes obtained by modifying or equivalently replacing the technical scheme of the present invention without creative results are within the protection scope of the present invention.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for describing specific embodiments and are not intended to limit the present invention.
[0038] The numerical values disclosed in the embodiments of the present invention are approximate values, not definite values. When the error or experimental conditions permit, all values within the error range may be included without being limited to the specific numerical values disclosed in the embodiments of the present invention.
[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0040] like Figure 1 As shown, this embodiment provides a production process for hot-rolled ribbed steel bar coils, and the systems involved in the production process include: a heating furnace 1, a high-pressure water descaling device 2, a roughing mill group 3, a No. 1 flying shear 4, a first intermediate rolling mill group 5, a No. 2 flying shear 6, a second intermediate rolling mill group 7, a pre-finishing rolling mill group 8, a pre-water cooling device 9, a No. 3 flying shear 10, a finishing rolling mill group 11, a water cooling device 12, a spinning machine 13, an air-cooled roller 14, and a P&F line 18 (accumulation type suspended conveyor), wherein the air-cooled roller 14 is equipped with a fan 15 and a heat preservation cover 16, and the product flowing out of the air-cooled roller 14 is transported to the P&F line 18 through a winding core rack 17.
[0041] in:
[0042] The heating furnace 1 is used to heat the blank.
[0043] The high-pressure water descaling device 2 is used for descaling; the roughing mill group 3 is used for roughing.
[0044] The No. 1 flying shear 1 is used for shearing the head and tail, and the first intermediate rolling mill group 5 is used for the first intermediate rolling.
[0045] The second flying shear 3 is used for shearing the head and tail, and the second intermediate rolling mill group 7 is used for the second intermediate rolling.
[0046] The pre-finishing rolling mill group 5 is used for pre-finishing rolling.
[0047] The pre-water cooling device 6 is used for water cooling.
[0048] The No. 3 flying shear 7 is used for shearing the head and tail, and the finishing mill group 8 is used for finishing rolling.
[0049] The water cooling device 9 is used for water cooling.
[0050] The spinning machine 10 is used for spinning and forming.
[0051] The air-cooled roller table 14 and the fan 15 and the heat-insulating cover 16 configured therein are used for air cooling and heat preservation.
[0052] The P&F line 18 is used for natural cooling, and the coiling core rack 17 is used to transport the wire rod to the P&F line 18 .
[0053] The production process includes the following steps:
[0054] S1. Select a square billet with chemical composition that meets the requirements for producing HRB400E hot-rolled ribbed steel bar coil as the billet, with a height × width × length of 165mm × 165mm × 12000mm, and heat the billet to 1040-1100°C, ensuring that the rolling temperature is 990-1020°C;
[0055] S2, the steel billet heated in step S1 is descaled by high-pressure water and then subjected to rough rolling to obtain a first round rolled piece, the first round rolled piece is sheared at the head and tail, and then subjected to intermediate rolling to obtain a second round rolled piece, the second round rolled piece is sheared at the head and tail, and then subjected to intermediate rolling again to obtain a third round rolled piece, and the third round rolled piece is subjected to pre-finish rolling to obtain a fourth round rolled piece;
[0056] The specific operations of this step are:
[0057] 1) rough rolling to obtain a first round rolled piece with a height×width of (76±0.5 mm)×(76±0.5 mm);
[0058] In this step, the rough rolling is carried out by a rough rolling mill composed of 6 rough rolling mills, and the hole types of the 6 rough rolling mills are box type-box type-box type-round type-elliptical type-round type. The material height × width of the 1st rolling mill is (108±1mm)×(164±1mm); the material height × width of the 2nd rolling mill is (118±1mm)×(122±1mm); the material height × width of the 3rd rolling mill is (83±1mm)×(126±1mm); the material height × width of the 4th rolling mill is (99±1mm)×(99±1mm); the material height × width of the 5th rolling mill is (63±1mm)×(121±1mm); the material height × width of the 6th rolling mill is (76±0.5mm)×(76±0.5mm);
[0059] 2) Then, the first round rolled piece is sheared at the head and tail, and then intermediate rolling is performed to obtain a second round rolled piece having a height×width of (36±0.5 mm)×(36±0.5 mm);
[0060] In this step, the intermediate rolling is carried out by an intermediate rolling mill group consisting of 6 intermediate rolling mills, and the hole types of the 6 intermediate rolling mills are elliptical-circular-elliptical-circular-elliptical-circular. The material height × width of the 7th rolling mill is (46±1mm)×(96±1mm); the material height × width of the 8th rolling mill is (58±1mm)×(58±1mm); the material height × width of the 9th rolling mill is (36±1mm)×(74±1mm); the material height × width of the 10th rolling mill is (46±1mm)×(46±1mm); the material height × width of the 11th rolling mill is (28±1mm)×(57±1mm), and the material height × width of the 12th rolling mill is (36±0.5mm)×(36±0.5mm);
[0061] 3) Then, the head and tail of the obtained second round rolled piece are sheared, and then the rolled piece is subjected to intermediate rolling again to obtain a third round rolled piece with a height×width of (29.5±0.5 mm)×(29.5±0.5 mm);
[0062] In this step, the intermediate rolling is carried out by an intermediate rolling mill composed of two intermediate rolling mills, and the pass types of the two intermediate rolling mills are elliptical-circular in sequence. The material height × width of the 13th rolling mill is (23±0.5mm)×(44±0.5mm); the material height × width of the 14th rolling mill is (29.5±0.5mm)×(29.5±0.5mm);
[0063] 4) Then, the third round rolled piece is subjected to pre-finish rolling, and the rolling speed of the pre-finish rolling is controlled at 10 m / s to 13 m / s, and a fourth round rolled piece having a height×width of (19±0.5 mm)×(19±0.5 mm) or a height×width of (23±0.5 mm)×(23±0.5 mm) is obtained through pre-finish rolling;
[0064] In this step, the pre-finishing rolling of φ6mm~φ8mm specifications is carried out by a pre-finishing rolling mill composed of 4 pre-finishing rolling mills, and the hole types of the 4 pre-finishing rolling mills are elliptical-circular-elliptical-circular in sequence. The material height×width of the 15th rolling mill is (18±0.5mm)×(35±0.5mm); the material height×width of the 16th rolling mill is (23±0.5mm)×(23±0.5mm); the material height×width of the 17th rolling mill is (16±0.5mm)×(27±0.5mm); the material height×width of the 18th rolling mill is (19±0.5mm)×(19±0.5mm). The pre-finishing rolling of φ10mm~φ12mm specifications is carried out by a pre-finishing rolling mill composed of 2 pre-finishing rolling mills, and the hole types of the 2 pre-finishing rolling mills are elliptical-circular in sequence. The material height × width of the 17-stand rolling mill is (18±0.5mm)×(35±0.5mm); the material height × width of the 18-stand rolling mill is (23±0.5mm)×(23±0.5mm);
[0065] S3, cooling the fourth round rolled piece through water to cool the temperature of the fourth round rolled piece to 860-900° C., then shearing the head and tail of the cooled fourth round rolled piece, and then finishing rolling to obtain a hot-rolled coil, then cooling the hot-rolled coil through water to cool the temperature of the hot-rolled coil to 960-1010° C., and spinning the cooled hot-rolled coil into a coil;
[0066] The specific steps are as follows:
[0067] 1) The obtained fourth round rolled piece is subjected to water cooling to cool the temperature of the fourth round rolled piece to 860-900° C.;
[0068] In this step, water cooling is carried out by a pre-water cooling device. The water pressure of the first stage pre-water cooling device is 0.60-0.80 MPa, and the water flow rate is 80-120 m3 / h; the water pressure of the second stage pre-water cooling device is 0.60-0.80 MPa, and the water flow rate is 80-120 m3 / h. The finishing rolling temperature of φ6mm-φ12mm specifications is controlled at 860-900℃.
[0069] 2) After cooling, the fourth round rolled piece is sheared at the head and tail, and then subjected to finish rolling to obtain a hot-rolled coil;
[0070] In this step, the φ6mm specification finishing rolling is carried out by a finishing mill composed of 10 finishing mills, and the hole types of the 10 finishing mills are elliptical-circular-elliptical-circular-elliptical-circular-elliptical-circular. The material height × width of the 19th rolling mill is (11.5±0.3mm)×(22±0.3mm); the material height × width of the 20th rolling mill is (14.5±0.3mm)×(14.5±0.3mm); the material height × width of the 21st rolling mill is (9.5±0.3mm)×(18±0.3mm); the material height × width of the 22nd rolling mill is (12±0.3mm)×(12±0.3mm); the material height × width of the 23rd rolling mill is (7.5±0.3mm)×(14.5±0.3mm) ; The material height × width of the 24th rolling mill is (9.5±0.3mm)×(9.5±0.3mm); the material height × width of the 25th rolling mill is (6±0.3mm)×(11.5±0.3mm); the material height × width of the 26th rolling mill is (7.5±0.3mm)×(7.5±0.3mm); the material height × width of the 27th rolling mill is (4.5±0.3mm)×(9.5±0.3mm); the material height × width of the 28th rolling mill is (6.0±0.1mm)×(6.0±0.1mm). The Φ8mm specification finishing rolling is carried out by a finishing mill composed of 8 finishing rolling mills. The hole types of the 8 finishing rolling mills are elliptical-circular-elliptical-circular-elliptical-circular-elliptical-circular. The height × width of the 21st rolling mill is (13.5 ± 0.3 mm) × (23 ± 0.3 mm); the height × width of the 22nd rolling mill is (15.5 ± 0.3 mm) × (15.5 ± 0.3 mm); the height × width of the 23rd rolling mill is (10.5 ± 0.3 mm) × (19 ± 0.3 mm); the height × width of the 24th rolling mill is (12.8 ± 0.3 mm) × (12.8 ± 0.3 mm ); 25 mills have a material height × width of (7.5±0.3mm) × (16±0.3mm); 26 mills have a material height × width of (10.1±0.3mm) × (10.1±0.3mm); 27 mills have a material height × width of (6.1±0.3mm) × (12.5±0.3mm); 28 mills have a material height × width of (8±0.1mm) × (7.5±0.1mm). φ10mm specification finishing rolling is carried out by a finishing mill consisting of 8 finishing mills, and the hole types of the 8 finishing mills are elliptical-circular-elliptical-circular-elliptical-circular-elliptical-circular.The height × width of the 21st rolling mill is (16±0.3mm)×(27±0.3mm); the height × width of the 22nd rolling mill is (20±0.3mm)×(20±0.3mm); the height × width of the 23rd rolling mill is (13±0.3mm)×(23±0.3mm); the height × width of the 24th rolling mill is (20±0.3mm)×(20±0.3mm); the height × width of the 25th rolling mill is (20±0.3mm)×(20±0.3mm); The height × width is (10±0.3mm) × (19.5±0.3mm); the height × width of the 26-stand mill is (12.5±0.3mm) × (12.5±0.3mm); the height × width of the 27-stand mill is (7.5±0.3mm) × (16.5±0.3mm); the height × width of the 28-stand mill is (10.1±0.1mm) × (10.1±0.1mm). The φ12mm specification finishing rolling is carried out by a finishing mill consisting of 6 finishing mills. The hole types of the 6 finishing mills are elliptical-circular-elliptical-circular-elliptical-circular. The height × width of the 21st rolling mill is (15±0.3mm)×(28±0.3mm); the height × width of the 22nd rolling mill is (18.5±0.3mm)×(18.5±0.3mm); the height × width of the 23rd rolling mill is (11.5±0.3mm)×(22.5±0.3mm); the height × width of the 24th rolling mill is (14.5±0.3mm)×(14.5±0.3mm); the height × width of the 25th rolling mill is (9.5±0.3mm)×(17.5±0.3mm); the height × width of the 26th rolling mill is (12±0.1mm)×(11.8±0.1mm).
[0071] 3) Then, the obtained hot-rolled coil is cooled by water to cool the temperature of the hot-rolled coil to 960-1010° C.;
[0072] In this step, water cooling is performed by a water cooling device. The water pressure of the first stage water cooling device is 0.60-0.80 MPa, and the water flow rate is 20-40 m3 / h; the water pressure of the second stage water cooling device is 0.60-0.80 MPa, and the water flow rate is 40-80 m3 / h; the water pressure of the third stage water cooling device is 0.60-0.80 MPa, and the water flow rate is 40-80 m3 / h; the water pressure of the fourth stage water cooling device is 0.60-0.80 MPa, and the water flow rate is 20-40 m3 / h. The spinning temperature of φ6mm-φ8mm specifications is controlled at 980-1010°C, and the spinning temperature of φ10mm-φ12mm specifications is controlled at 960-980°C.
[0073] 4) Then the cooled hot rolled coil is spun into coil;
[0074] In this step, the spinning forming is carried out by a spinning machine, the leading coefficient of the spinning machine is 1.010-1.025, the swing positive amplitude coefficient is 0.02, the swing positive amplitude coefficient is 0.02, and the swing time is 8 seconds.
[0075] 5) Then, the obtained coils are cooled by a fan to cool the coils to a temperature below 700°C; in this step, the cooling is performed by a cooling roller. There are 12 Stelmor fans, φ6mm
[0076] Specification 1# fan opens 70% air volume, 2# fan opens 50% air volume; φ8mm specification 1# fan opens 80% air volume, 2# fan opens 60% air volume, 4# fan opens 50% air volume; φ10mm specification 1# fan opens 80% air volume, 2# fan opens 80% air volume, 3# fan opens 50% air volume, 4# fan opens 50% air volume, 5# fan opens 50% air volume, 6# fan opens 50% air volume; φ12mm specification 1# fan opens 80% air volume, 2# fan opens 80% air volume, 3# fan opens 80% air volume, 4# fan opens 80% air volume, 5# fan opens 60% air volume, 6# fan opens 60% air volume; air-cooled roller table total 11 sections, roller speed of section 1 is 0.45-0.48m / s; roller speed of section 2 is 0.48-0.51m / s; roller speed of section 3 is 0.51-0.54m / s; roller speed of section 4 is 0.54-0.57m / s; roller speed of section 5 is 0.57-0.60m / s; roller speed of section 6 is 0.60-0.63m / s; roller speed of section 7 is 0.63-0.66m / s; roller speed of section 8 is 0.66-0.70m / s; roller speed of section 9 is 0.70-0.75m / s; roller speed of section 10 is 0.70-0.75m / s; roller speed of section 11 is 0.80-0.85m / s; there are 15 thermal insulation covers in total, and all the thermal insulation covers are opened.
[0077] 6) Then the cooled coils are collected by the lower coiler, and the coils are placed on the C-hook by a coil transport trolley and transported to the P&F line for natural cooling. The natural cooling time is 30 to 40 minutes, and the finished product is obtained after cooling.
[0078] The production process of the hot-rolled ribbed steel bar coil provided in this embodiment adopts a high-V and low-Si, Mn chemical composition formula to solve the problem of rising prices of ferrosilicon and silicon-manganese alloys through reasonable design of alloy composition and rolling process structure. This formula can achieve stable performance and low-cost production of hot-rolled ribbed steel bar coils, greatly reducing alloy costs, and achieving grain refinement, uniform structure, high maximum force total elongation, and improved performance of the hot-rolled ribbed steel bar coils, bringing huge economic and social benefits to the enterprise.
[0079] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A production process for hot-rolled ribbed steel bar coils, It is characterized in that The steps include: S1. Use a square billet with a chemical composition of C: 0.21-0.25%, Si: 0.20-0.35%, Mn: 1.10-1.35%, P≤0.040%, S≤0.040%, V: 0.020-0.030%, Ceq: 0.41-0.49% as the billet, and heat the billet to 1040-1100°C to ensure the rolling start temperature is 990-1020°C; S2, descaling the heated steel billet with high-pressure water and then performing rough rolling to obtain a first round rolled piece, shearing the first round rolled piece at the head and tail, and then performing intermediate rolling to obtain a second round rolled piece, shearing the second round rolled piece at the head and tail, and then performing intermediate rolling again to obtain a third round rolled piece, and performing pre-finish rolling on the third round rolled piece to obtain a fourth round rolled piece; S3, water-cooling the fourth round rolled piece to cool the temperature of the fourth round rolled piece to 860-900°C, then shearing the cooled fourth round rolled piece at the head and tail, and then finishing rolling to obtain a hot-rolled coil, then water-cooling the hot-rolled coil to cool the temperature of the hot-rolled coil to 960-1010°C, and spinning the cooled hot-rolled coil into a coil.
2. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S3, the specification range of the hot-rolled coil is φ6 mm to φ12 mm, and the chemical composition ratios of each specification are as follows: φ6㎜ specification, C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.05~1.15%, P≤0.040%, S≤0.040%, V: 0.020~0.025%, Ceq: 0.41~0.46%; φ8mm—φ10㎜ specifications, C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.15~1.25%, P≤0.040%, S≤0.040%, V: 0.020~0.025%, Ceq: 0.42~0.47%; φ12㎜Specifications: C: 0.21~0.25%, Si: 0.20~0.35%, Mn: 1.20~1.35%, P≤0.040%, S≤0.040%, V: 0.025~0.030%, Ceq: 0.43~0.49%.
3. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S2, The rough rolling is carried out by a rough rolling mill consisting of 6 rough rolling mills, and the pass types of the 6 rough rolling mills are box type-box type-box type-round type-elliptical type-round type; The first intermediate rolling is carried out by an intermediate rolling mill consisting of 6 intermediate rolling mills, and the hole types of the 6 intermediate rolling mills are elliptical-circular-elliptical-circular-elliptical-circular; The second intermediate rolling is carried out by an intermediate rolling mill consisting of two intermediate rolling mills, and the hole types of the two intermediate rolling mills are elliptical-circular respectively.
4. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S2, the rolling speed of the pre-finish rolling is controlled at 10 m / s to 13 m / s.
5. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S2, To produce coils with a specification of φ6mm to φ8mm, the pre-finishing rolling is carried out by a pre-finishing rolling mill consisting of 4 pre-finishing rolling mills. The hole types of the 4 pre-finishing rolling mills are elliptical-circular-elliptical-circular in sequence. For producing coils with specifications of φ10mm to φ12mm, the pre-finishing rolling is carried out by a pre-finishing rolling mill consisting of two pre-finishing rolling mills, and the hole types of the two pre-finishing rolling mills are elliptical and circular respectively.
6. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S3, To produce φ6mm hot-rolled coil, the finishing rolling is carried out by a finishing mill consisting of 10 finishing mills. The hole types of the 10 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular-oval-circular; To produce φ8mm hot-rolled coils, the finishing rolling is carried out by a finishing mill consisting of 8 finishing mills. The hole types of the 8 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular; To produce φ10mm hot-rolled coils, the finishing rolling is carried out by a finishing mill consisting of 8 finishing mills. The hole types of the 8 finishing mills are oval-circular-oval-circular-oval-circular-oval-circular-oval-circular. For producing φ12mm hot-rolled coil, finishing rolling is carried out by a finishing mill consisting of 6 finishing mills, and the hole types of the 6 finishing mills are elliptical-circular-elliptical-circular-elliptical-circular.
7. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S3, water cooling is carried out by a water cooling device, the water pressure of the first water cooling device is 0.60-0.80MPa, and the water flow rate is 20-40m3 / h; the water pressure of the second water cooling device is 0.60-0.80MPa, and the water flow rate is 40-80m3 / h; the water pressure of the third water cooling device is 0.60-0.80MPa, and the water flow rate is 40-80m3 / h; the water pressure of the fourth water cooling device is 0.60-0.80MPa, and the water flow rate is 20-40m3 / h, wherein the spinning temperature for producing φ6mm-φ8mm specifications is controlled at 980-1010°C, and the spinning temperature for producing φ10mm-φ12mm specifications is controlled at 960-980°C.
8. The production process of hot-rolled ribbed steel bar coil according to claim 1, It is characterized in that In step S3, the spinning forming is carried out by a spinning machine, the leading coefficient of the spinning machine is 1.010-1.025, the positive amplitude coefficient of the swing is 0.02, the positive amplitude coefficient of the swing is 0.02, and the swing time is 8 seconds.
9. The production process of hot-rolled ribbed steel coil according to claim 1, It is characterized in that In step S3, the coiled conch after spinning is air-cooled by an air-cooled roller, and the air-cooled roller has 11 sections, with a roller speed of 0.45-0.48 m / s in section 1, 0.48-0.51 m / s in section 2, 0.51-0.54 m / s in section 3, 0.54-0.57 m / s in section 4, 0.57-0.60 m / s in section 5, 0.60-0.63 m / s in section 6, 0.63-0.66 m / s in section 7, 0.66-0.70 m / s in section 8, and 0.70-0.75 m / s in section 9. 10-section roller speed 0.70-0.75m / s; The speed of the 11-section rollers is 0.80-0.85 m / s; and there are 15 insulation covers in the air cooling process, and all the insulation covers are opened.
10. A steel bar coil produced by the production process of hot-rolled ribbed steel bar coil according to any one of claims 1 to 9.
Citation Information
Patent Citations
Finish-pass-sharing production method of plain round hot-rolled steel bars with diameter being 6.5 mm and disc screw hot-rolled steel bars with diameter being 6 mm
CN104117536A
Production technology for HRB400 coiled fine-grain reinforcing steel bar
CN106319179A
Production method of hot rolled ribbed steel bar
CN111394560A
Q195 cold forging steel production process
CN113333463A
Method for reducing HRB400E oxidation burning loss of low-Si hot-rolled ribbed steel bar and HRB400E hot-rolled ribbed steel bar
CN114959467A