Corrosion-resistant alloy seamless tube and manufacturing process and application thereof

The treatment of Hastelloy B3 alloy through the hot extrusion process solves the difficulty of making seamless pipes, significantly improves the bending, torsional and corrosion resistance of the alloy, meets the comprehensive performance requirements of the pipe, and achieves corrosion resistance High quality manufacturing of alloy seamless tubes.

CN118926349APending Publication Date: 2024-11-12JIANGSU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411071057.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Due to its high degree of improvement, high resistance to thermal processing deformation, severe cold work hardening and easy precipitation of harmful phases in Hastelloy B3 alloy, it is difficult to make seamless pipes. There is a lack of reports on the manufacturing process of its seamless pipes in China, which is difficult to meet. Industry has high requirements for the comprehensive performance of metal pipes.

Method used

The process of Hastelloy B3 alloy is processed using the hot extrusion process, including smelting, forging, hot extrusion, pickling and inspection. Through vacuum induction and self-consumption processes, smelting, homogenizing heat treatment, upsetting and then drawing forging, heat Extrusion and sulfuric acid-nitric acid-hydrofluoric acid pickling improve the strength and corrosion resistance of the alloy.

Benefits of technology

It significantly enhances the bending and torsion resistance of Hastelloy B3 alloy, ensures the mechanical properties of corrosion-resistant alloy seamless pipes, and meets the strict requirements of dimensional accuracy and surface quality, and has good practicality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926349A_ABST
    Figure CN118926349A_ABST
Patent Text Reader

Abstract

The invention provides a corrosion-resistant alloy seamless pipe and a manufacturing process and application thereof, and belongs to the technical field of pipe preparation and hot extrusion. According to the manufacturing process, the Hastelloy B3 alloy is treated through the hot extrusion process, so that the corrosion-resistant alloy seamless pipe is manufactured, the manufacturing process is reasonable in material use and scientific in proportion, the overall strength can be improved to the maximum extent by matching with a refining agent, the overall bending resistance and the overall torsion resistance are greatly improved, and the mechanical property of the corrosion-resistant alloy is effectively ensured; the corrosion-resistant alloy seamless pipe manufactured by the manufacturing process meets the strict requirements of the pipe on the size precision, the surface quality and the forming process, and has good practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipe preparation and hot extrusion, and specifically relates to a corrosion-resistant alloy seamless pipe and a manufacturing process and application thereof. Background Art

[0002] Hastelloy B3 has a high degree of alloying (especially Mo element), has high resistance to hot working deformation, severe cold working hardening, and easy precipitation of harmful phases during heat treatment. Therefore, it is very difficult to use Hastelloy B3 alloy to manufacture seamless pipes. At present, domestic research on Hastelloy B3 alloy is limited to the introduction of its performance characteristics, the introduction of pressure vessel and heat exchanger manufacturing technology, and the research on welding process, forming process, and corrosion resistance. There are few reports on the manufacturing process of seamless pipes of this alloy. Hastelloy B3 alloy itself is extremely corrosion-resistant. With the development of industrial technology, the complexity of environmental media, and the intensification of international competition, many industries have higher and higher requirements for the comprehensive performance of metal pipes. Therefore, it is necessary to develop a method for preparing corrosion-resistant alloy seamless pipes using Hastelloy B3 alloy. Summary of the invention

[0003] In view of some deficiencies in the prior art, the present invention provides a corrosion-resistant alloy seamless pipe and a manufacturing process and application thereof; the present invention adopts a hot extrusion process to process the Hastelloy B3 alloy to manufacture the corrosion-resistant alloy seamless pipe, the manufacturing process uses reasonable materials and scientific proportions, and the combination of refining agents can maximize the overall strength, greatly enhance the overall bending and torsional properties, and effectively ensure the mechanical properties of the corrosion-resistant alloy; the corrosion-resistant alloy seamless pipe manufactured under the manufacturing process meets the strict requirements of the pipe for dimensional accuracy, surface quality and forming process, and has good practicality.

[0004] In order to achieve the above technical objectives, the present invention adopts the following technical means:

[0005] The present invention first provides a manufacturing process for a corrosion-resistant alloy seamless pipe, the manufacturing process comprising:

[0006] (1) Smelting: The untreated Hastelloy B3 alloy is smelted by vacuum induction + vacuum consumable process to produce qualified hollow ingots;

[0007] (2) Forging: The hollow ingot is subjected to homogenization heat treatment, and then the consumable ingot is subjected to homogenization forging. Then, the ingot is pre-deformed by upsetting and stretching, and then stretched and forged into an intermediate billet;

[0008] (3) Hot extrusion: The intermediate billet is surface cleaned and preheated, and then the surface oxide scale and other harmful defects are removed, and then hot extrusion is performed on a high-performance hot extruder to obtain Hastelloy B3 rough pipe;

[0009] (4) Pickling: Straighten the Hastelloy B3 rough pipe, cut off the head and tail defects and remove the burrs, and then pickle it with sulfuric acid and nitric acid-hydrofluoric acid in sequence. After pickling, a stainless steel pipe is obtained;

[0010] (5) Initial polishing: The obtained stainless steel pipe is inspected and polished inside and outside, and then polished inside and outside to obtain a finished pipe;

[0011] (6) Inspection: ultrasonic inspection is performed on each of the finished tubes to obtain the corrosion-resistant alloy seamless tube.

[0012] Preferably, in step (2), the homogenization heat treatment is carried out at 1170-1190° C. for 25 hours.

[0013] Preferably, in step (2), the homogenization forging step is to perform homogenization forging of consumable ingots using a fast forging machine and a fine forging machine, and the fast forging machine forges the pliers handle and then performs pre-deformation by upsetting and then drawing.

[0014] Preferably, in step (2), the total forging elongation coefficient is not less than 3, the head resection rate is 4%, and the tail resection rate is 6%.

[0015] Preferably, in step (3), the hot extrusion operation comprises:

[0016] The hot extrusion is carried out on a 60MN horizontal hot extruder at a temperature ranging from 1150 to 1200°C, and a hot extruded rough tube is obtained after the extrusion is completed; the extrusion speed is 120 to 180 mm / s, so that the excess thickness of the intermediate billet is controlled at 5 to 20 mm.

[0017] Preferably, in step (4), the concentration of the sulfuric acid solution is 16 wt %, and the conditions for sulfuric acid pickling are soaking at a temperature of 165° F for 3 minutes.

[0018] Preferably, in step (4), the nitric acid-hydrofluoric acid is a mixed solution of 8 wt % HNO 3 and 3 wt % HF, and the conditions for immersion pickling in the nitric acid-hydrofluoric acid are immersion at a temperature of 145° F for 25 minutes.

[0019] The present invention also provides a corrosion-resistant alloy seamless pipe manufactured by the above method, wherein the matrix of the corrosion-resistant alloy seamless pipe is equiaxed austenite grains, and the average grain sizes in the transverse and longitudinal directions are both level 7.

[0020] The present invention also provides application of the corrosion-resistant alloy seamless pipe in the fields of petroleum transportation and nuclear power.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention uses reasonable materials and has a scientific ratio. The overall strength can be improved to the maximum extent by combining with a refining agent, so that the obtained pipe has excellent strength and better corrosion resistance. By calculating a suitable stretching ratio for stretching, the overall bending and torsion resistance is greatly enhanced, and the mechanical properties of the Hastelloy B3 alloy are effectively ensured. The technical steps are more reasonable. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a graph showing the relationship between the tensile properties and temperature of corrosion-resistant alloy seamless pipes. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto. It is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features known in the art are not described.

[0025] Example 1: Production of corrosion-resistant alloy seamless pipe

[0026] (1) Smelting:

[0027] The untreated Hastelloy B3 alloy was smelted by vacuum induction + vacuum consumable process to produce qualified hollow ingots. That is, firstly, a 450mm ingot was cast by vacuum induction smelting, and then vacuum consumable remelting was performed to finally obtain a 550mm homogenized ingot.

[0028] (2) Forging: The hollow ingot is kept at 1170-1190℃ for 25h for homogenization heat treatment. After the heat treatment, it is cooled to room temperature to eliminate the segregation in the cast structure and improve the plasticity and uniformity of the material. Then the consumable ingot is homogenized forged by a fast forging machine and a precision forging machine. After the fast forging machine forges the pliers, it is pre-deformed by upsetting and stretching, and then homogenized heat treatment is performed. The total elongation coefficient of forging is not less than 3.5, and the final forging is a 230mm Φ intermediate billet, with the head and tail removal rates greater than 4% and 6% respectively, to ensure the quality of the final product.

[0029] (3) Hot extrusion:

[0030] The surface of the 230mm intermediate billet is cleaned and preheated, and the preheating temperature is determined according to the alloy characteristics and the extruder capacity. The surface of the forged alloy round tube billet is peeled to remove the surface oxide scale and other harmful defects, and its size is controlled to Φ213mm±0.5mm, and the surface roughness Ra is controlled below 1.6μm; hot extrusion operation is carried out on a high-performance hot extruder. Through reasonable die design and process parameter control, the temperature is hot extruded in the range of 1150-1200℃, and the extrusion speed is 120-180mm / s so that the residual thickness of the intermediate billet is controlled to 5-20mm, and the Hastelloy B3 pipe with the required cross-sectional shape and size is obtained. The pipe specification after extrusion is Ф125×8mm, and the Hastelloy B3 rough pipe is obtained.

[0031] (4) Pickling:

[0032] The Hastelloy B3 rough pipe is straightened, the defects at the head and tail are cut off, and the burrs are removed. Then, it is pickled by immersion in sulfuric acid and nitric acid-hydrofluoric acid in sequence. After the pickling, a stainless steel pipe is obtained; wherein, the sulfuric acid is soaked at a temperature of 165℉ for 3 minutes, and the nitric acid-hydrofluoric acid is soaked at a temperature of 145℉ for 25 minutes. The sulfuric acid solution is 16wt% H2SO4, and the nitric acid solution is 8wt% HNO3 and 3wt% HF.

[0033] (5) First throw:

[0034] The pipe is washed with high-pressure water to remove residual acid, and the surface is ground and polished to obtain a finished pipe, namely the corrosion-resistant alloy seamless pipe.

[0035] (6) Inspection:

[0036] The finished tubes are inspected one by one by ultrasonic, and the size of artificial defects of the ultrasonic inspection standard sample is 0.04mm×3mm×0.08mm (depth×length×width).

[0037] Each finished pipe is inspected for size and surface. The allowable deviations of the outer diameter and wall thickness are controlled within ±0.04mm, and the allowable deviation of the wall thickness is ±0.03mm; the inner surface roughness Ra≤0.9μm, and the outer surface roughness Ra≤0.7μm.

[0038] Physical and chemical inspection: According to ASTM E 8 / E 8M-2021 "Metallic Materials Tensile Test Methods" and ASTM E 21-2020 "High-temperature Tensile Test Methods for Metallic Materials", a DDL-300 electronic universal tensile testing machine was used to conduct a tensile test at 25-525°C, and the tensile strength Rm, yield strength Rp0.2 and elongation A50 were recorded; according to ASTM E 92-2017 "Standard Test Methods for Vickers Hardness and Knoop Hardness of Metallic Materials", a 570HAD digital display Brinell hardness tester was used to test the Vickers hardness of the cross section. The test results are as follows: Figure 1 And as shown in Table 1.

[0039] (7) Cleaning and packaging:

[0040] Cleaning: Use solvents such as acetone or alcohol to thoroughly clean the inner and outer surfaces of the pipe to ensure that there is no oil or foreign matter.

[0041] Packaging: Use appropriate packaging materials (such as pentachloroethylene plastic bags and wooden boxes) to properly package the pipes and attach barcode labels to facilitate traceability and management.

[0042] Figure 1 The relationship between the tensile properties and temperature of the corrosion-resistant alloy seamless pipe is shown in the figure. It can be seen from the figure that in the range of 25-525℃, with the increase of temperature, the tensile strength and yield strength of the Hastelloy B3 alloy pipe gradually decrease, among which the tensile strength decreases faster first and then slower, and the yield strength decreases uniformly and slowly; the elongation at 25-525℃ shows a trend of first decreasing, then increasing, and then decreasing with the increase of temperature; at 25℃, the plasticity is good, and the elongation at break reaches 59.5%. When the temperature rises to 100℃, the elongation at break decreases, and the elongation at break begins to rise as the temperature continues to rise, until it reaches 59.0% at 300℃. When the temperature increases further, the elongation at break begins to decrease again, until it reaches the minimum value of 51.0% at 525℃. It can be seen that the Vickers hardness of the Hastelloy B3 alloy seamless pipe matrix is ​​about 221HV30, which has good mechanical properties.

[0043] Table 1. Physical and chemical test results of corrosion-resistant alloy seamless pipes

[0044] Yield Strength tensile strength Elongation after fracture Rockwell hardness Corrosion rate Example 1 820 516 48 92 0.032 Prior art 615 369 37 55 4.2

[0045] It can be seen from Table 1 that, compared with the prior art, the corrosion-resistant alloy seamless pipe produced by the method of the present invention has better mechanical properties and corrosion resistance.

[0046] In summary, the manufacturing process uses reasonable materials and scientific proportions, and the combination of refining agents can maximize the overall strength, greatly enhance the overall bending and torsional properties, and effectively ensure the mechanical properties of the corrosion-resistant alloy; the corrosion-resistant alloy seamless pipe manufactured under the manufacturing process meets the strict requirements of the pipe for dimensional accuracy, surface quality and forming process, and has good practicality.

[0047] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.

Claims

1. A manufacturing process for a corrosion-resistant alloy seamless pipe, characterized in that: The manufacturing process comprises: (1) Smelting: The untreated Hastelloy B3 alloy is smelted by vacuum induction + vacuum consumable process to produce qualified hollow ingots; (2) Forging: The hollow ingot is subjected to homogenization heat treatment, and then the consumable ingot is subjected to homogenization forging. Then, the ingot is pre-deformed by upsetting and stretching, and then stretched and forged into an intermediate billet; (3) Hot extrusion: The intermediate billet is surface cleaned and preheated, and then the surface oxide scale and other harmful defects are removed, and then hot extrusion is performed on a high-performance hot extruder to obtain Hastelloy B3 rough pipe; (4) Pickling: Straighten the Hastelloy B3 rough pipe, cut off the head and tail defects and remove the burrs, and then pickle it with sulfuric acid and nitric acid-hydrofluoric acid in sequence. After pickling, a stainless steel pipe is obtained; (5) Initial polishing: The obtained stainless steel pipe is inspected and polished inside and outside, and then polished inside and outside to obtain a finished pipe; (6) Inspection: ultrasonic inspection is performed on each of the finished tubes to obtain the corrosion-resistant alloy seamless tube.

2. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (2), the homogenization heat treatment is carried out at 1170-1190° C. for 25 hours.

3. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (2), the homogenization forging step is to use a fast forging machine and a fine forging machine to perform homogenization forging of the consumable ingot, and the fast forging machine forges the pliers handle and then uses an upsetting and then drawing method to perform pre-deformation.

4. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (2), the total forging elongation coefficient is not less than 3, the head resection rate is 4%, and the tail resection rate is 6%.

5. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (3), the hot extrusion operation includes: The hot extrusion is carried out on a 60MN horizontal hot extruder at a temperature ranging from 1150 to 1200°C, and a hot extruded rough tube is obtained after the extrusion is completed; the extrusion speed is 120 to 180 mm / s, so that the excess thickness of the intermediate billet is controlled at 5 to 20 mm.

6. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (4), the concentration of the sulfuric acid solution is 16 wt %, and the conditions for sulfuric acid pickling are soaking at a temperature of 165° F for 3 minutes.

7. The manufacturing process of the corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In step (4), the nitric acid-hydrofluoric acid is a mixed solution of 8 wt % HNO 3 and 3 wt % HF, and the conditions for immersion pickling in the nitric acid-hydrofluoric acid are immersion at a temperature of 145° F for 25 minutes.

8. The corrosion-resistant alloy seamless pipe manufactured by the method according to any one of claims 1 to 7, characterized in that: The matrix of the corrosion-resistant alloy seamless pipe is equiaxed austenite grains, and the average grain sizes in the transverse and longitudinal directions are both grade 7.

9. Application of the corrosion-resistant alloy seamless pipe according to claim 8 in the fields of petroleum transportation and nuclear power.

Citation Information

Patent Citations

  • GH3600 alloy fine thin-walled seamless pipe manufacturing method

    CN103962411A

  • High-corrosion-resistance nickel-copper alloy seamless pipe and manufacturing method thereof

    CN105331850A

  • Method for thermally extruding and deforming high-temperature alloy Inconel 625 pipe through short process

    CN105331913A

  • Manufacturing method of high silicon titaniferous austenitic stainless steel cladding pipe

    CN109013744A

  • Ni-Mo corrosion-resistant alloy seamless tube for corrosion-resistant device and manufacturing method of Ni-Mo corrosion-resistant alloy seamless tube

    CN115161515A