Spinning and material adding integrated forming method for large-diameter-thickness-ratio thin-wall inner container part
By using mobile heating devices and spinning technology in the spinning press, combined with additive manufacturing, the problem of wrinkling and cracking of large diameter and thin wall inner liner parts during spin forming is solved, achieving high quality and high efficiency The spin forming avoids waste of materials and weld problems.
Patent Information
- Application Number
- CN202411064670.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Large diameter and thickness are more likely to cause wrinkles and cracks during spin forming, and the prior art are caused by many processes and poor quality, or the cylinder billet is costly and material waste is serious.
The heating device is used to move on the longitudinal slide plate or spindle box of the spinner machine, synchronously with the rotary wheel, and after each passage of shrinking diameter, the heating device moves radially to the cylinder blank to maintain the temperature of the forming area, and combine the spinning pressure. Achieve integrated formation with additive manufacturing.
It avoids multiple welds and material waste, improves the overall strength and appearance quality of the parts, realizes automated control and accurate temperature management, and overcomes the problem of spin-sealing sealing of thin-walled cylindrical parts.
Smart Images

Figure CN118926389A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of plastic processing and forming, and in particular to a method for integrally forming a thin-walled liner component with a large diameter-to-thickness ratio by spinning and additive manufacturing. Background Art
[0002] For parts with large diameter-to-thickness ratio such as water heater liner, low-pressure gas cylinder parts, and engine housings and missile housings in the aerospace field, the processing method is usually to stamp the two ends, roll and weld the middle into a tube, and then weld them into a whole. Or the method of using a seamless tube blank to spin by a pendulum wheel is adopted. The former has poor quality due to many processes and many welds, while the latter has high cost of the tube blank and serious thickening of the forming section during spinning, resulting in material waste.
[0003] However, when using a large diameter-to-thickness ratio cylindrical blank for shrink spinning, due to the large diameter and small wall thickness of the cylindrical blank, defects such as wrinkling and cracking are very likely to occur during the shrink spinning process, making the forming difficult. At the same time, large diameter cylindrical blanks usually need to be curled and welded by cold-rolled plates, and the weld is very likely to crack during processing, making the forming difficulty of the large diameter-to-thickness ratio liner further increased. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned problem of integrated spinning forming of an inner liner with or without welds and with a large diameter-to-thickness ratio, and to provide a method for integrated spinning and additive forming of a thin-walled inner liner with a large diameter-to-thickness ratio.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for forming a large diameter-to-thickness ratio thin-walled liner by spinning additive integration, wherein a heating device is clamped on a longitudinal slide plate or a spindle box of a spinning machine, and the heating device is synchronized with the spinning wheel in the axial direction during spinning of the tube blank, and can independently move radially toward the tube blank; the specific forming process includes the following steps:
[0007] S1. The tube blank is clamped on the spindle; the heating device is installed on the longitudinal slide or the spindle box and moves back and forth along the axial direction to heat the area of the tube blank to be spun to the temperature required for forming;
[0008] S2. The spinning wheel performs multiple passes of alternate reciprocating shrinking and spinning of the tube blank, and after each pass of shrinking and spinning, the heating device is moved radially toward the tube blank by an optimal sensing distance, so that the temperature of the tube blank forming area is maintained in the desired temperature range;
[0009] S3. After the first end of the tube blank is compressed to the required mouth size, the tube blank is turned around and clamped, so that the second end is gradually compressed into a flat bottom with a hole, and then additive manufacturing is performed on the hole to achieve bottom sealing.
[0010] The heating device is an induction coil, a flame spray gun or a laser heater;
[0011] When induction heating is performed by an induction coil, the induction coil is installed on one side of the spindle box and is individually controlled by a guide rail-slider device, and is driven by a motor to move closer to or away from the barrel in the vertical direction.
[0012] When a flame spray gun is used for heating, a single-head or multi-head flame spray gun can be used according to the required temperature for heating the tube blank. The flame spray gun is installed on one side of the longitudinal slide of the machine tool and moves axially and close to the tube blank with the longitudinal slide of the machine tool, or it is installed separately on one side of the spindle box and controlled separately by a guide rail-slider device.
[0013] When a laser heater is used for heating, the laser head of the laser heater is installed on one side of the longitudinal slide of the machine tool and moves axially and approaches the tube blank with the longitudinal slide of the machine tool, or is installed separately on one side of the spindle box and is controlled separately by a guide rail-slider device.
[0014] The axial position of the heating device is located outside the rotating wheel, that is, located in the end side area of the tube blank to be formed.
[0015] During each spinning process, the moving distance of the heating device toward the tube blank should maintain the required temperature range of the material in the area to be formed of the tube blank.
[0016] Additive manufacturing includes any one of arc additive, electron beam fuse, and laser additive.
[0017] Single-wheel spinning or double-wheel spinning is used in the shrinking spinning process.
[0018] Compared with the prior art, the present invention has the following advantages and effects:
[0019] (1) It can avoid stamping and welding of multiple parts, which is beneficial to reduce welds and thus improve the overall strength and appearance quality of parts.
[0020] (2) Heating equipment such as flame spray guns, induction coils, and laser heaters are installed on the longitudinal slide of the machine tool and can move in the vertical direction, achieving stable heating when the diameter of the tube billet changes significantly during the forming process. This overcomes the difficulty of separate coordinated control of the heating device and the forming tool and the limitation that the induction coil is only suitable for heating tube billets with equal diameters, and is conducive to the realization of automated control of hot shrink spinning.
[0021] (3) When flame spray gun or laser heating is used, the heating device moves synchronously with the rotary wheel in each pass; when induction heating is used, the radial position of the heating device can be adjusted in each pass according to parameters such as the spindle speed, the rotary wheel feed speed and the reduction amount of the previous pass to obtain the optimal distance between the heating device and the part to be formed, thereby more accurately controlling the forming temperature of the tube blank.
[0022] (4) The spinning wheel does not need to swing during multi-pass spinning, which reduces the complexity of the equipment tooling and control system and avoids material waste caused by increased wall thickness in the reduced diameter forming section.
[0023] (5) Combining spinning with additive manufacturing avoids longitudinal or circumferential welds and overcomes the difficulty of spinning and sealing thin-walled cylindrical parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a process flow chart of the invention's large diameter-to-thickness ratio thin-walled liner spin-formed additive integrated forming process.
[0025] Figure 2 This is a rough workpiece of a thin-walled liner with a large diameter-to-thickness ratio according to an embodiment of the present invention, wherein: a cylinder blank 1, an induction coil 21, and two rotating wheels 31, 32.
[0026] Figure 3 This is the inner liner target part described in the embodiment of the present invention.
[0027] Figure 4 It is a schematic diagram of the initial vertical position of the induction coil before the double-wheel spinning of the present invention.
[0028] Figure 5 This is a front view of the radial eccentric position of the induction coil during double-wheel spinning of the present invention.
[0029] Figure 6 It is a side view of the radial eccentric position of the induction coil during the double-wheel spinning of the present invention.
[0030] Figure 7 This is a front view of a concentric heating position of an induction coil to be avoided by the present invention.
[0031] Figure 8 This is a side view of a concentric heating position of an induction coil to be avoided by the present invention.
[0032] Fig. 9 This is the process of arc material addition of the present invention.
[0033] Fig.10 It is a schematic diagram of the initial position of the flame spray gun before the single-wheel spinning of the present invention.
[0034] Fig.11 This is a front view of the radial position of the flame spray gun during single-wheel spinning of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with specific embodiments.
[0036] Example
[0037] The outer diameter of the cylindrical part with large diameter-to-thickness ratio is 220mm, the wall thickness is 1.4mm, and the diameter-to-thickness ratio is greater than 150 (see Figure 2 ), made of SPCC cold-rolled steel sheets. Figure 3 As shown in the figure, the narrowest diameter of the closing port is 76mm. The other end is spun flat by reducing the diameter, and then the bottom is sealed by additive manufacturing. Figure 1 The method of the present invention is shown as being formed by heat shrinking and spinning.
[0038] This embodiment adopts double-wheel spinning. Before processing, a single-turn induction coil with a diameter of 240 mm is installed on one side of the spindle box. The servo motor drives the induction coil to move in the vertical direction and axial direction. In this embodiment, the induction coil 21 is sleeved on the tube blank 1 between the two spinning wheels 31 and 32. The axial position of the induction coil 21 is located outside the spinning wheel 31, that is, close to the end of the tube blank to be formed. Figure 2 .
[0039] The spinning steps are as follows:
[0040] (1) The tube blank 1 is clamped on the main shaft, and the induction coil 21 is arranged concentrically with the tube blank 1, as shown in FIG. Figure 4 shown.
[0041] (2) Start the main shaft and rotate it at a low speed of 100 r / min. Move the induction coil 21 back and forth with the longitudinal slide at a speed of 50 mm / s until the part of the tube to be formed is heated to 600±10°C.
[0042] (3) Increase the spindle speed to 350 r / min, perform multiple passes of alternating back and forth spinning with a pass reduction of 3 mm and a spinning wheel feed ratio of 2.8 mm / r. After each pass, press the induction coil 21 Figure 5 , 6 The vertical direction is moved by 2.5 mm to control the temperature of the part to be formed within the range of 500-600° C. until the spinning forming of one end of the tube blank 1 is completed.
[0043] If the induction coil 21 is always kept concentric with the tube blank 1 during the multi-pass spinning process, Figure 7 , 8 The improperly heated area shown is that since the induction coil is closest to position A, the temperature of the annular area at position A is higher, while the annular area at position B to be formed cannot reach the specified forming temperature in time because it is far away from the induction coil.
[0044] (4) Remove the workpiece and turn it around to clamp it on the spindle. Repeat steps (2) and (3) to shrink the other end of the tube blank and spin it to a small hole of 4±0.5 mm (see Fig. 9 Small hole diagram) and ensure that the bottom is flat.
[0045] (5) The small hole is sealed by arc additive to achieve the bottom sealing of the inner liner, and the integrated forming of the inner liner with a large diameter-to-thickness ratio is completed. Fig. 9 , where 4 is an arc fuse welding gun.
[0046] If the double spinning wheel is changed to a single spinning wheel 3 for spinning, the induction coil 21 is replaced with a flame spray gun 22, and the flame spray gun 22 is installed on the longitudinal slide of the machine tool. The flame spray gun 22 can move axially and radially with the longitudinal slide, such as Fig.10 shown.
[0047] In this embodiment, the process parameters of multi-pass spinning are the same as those in Example 1, namely: the spindle speed is 350 r / min, the pass reduction is 3 mm, the spinning wheel feed ratio is 2.8 mm / r, and after each pass, the flame spray gun 22 moves synchronously with the longitudinal slide of the bed and the spinning wheel in the radial direction. Fig.10 shown.
[0048] As described above, the present invention can be better implemented.
[0049] The implementation methods of the present invention are not limited to the above-mentioned embodiments, and any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for forming a large diameter-to-thickness ratio thin-walled liner by spinning additive, characterized in that The heating device is clamped on the longitudinal slide plate or the spindle box of the spinning machine. When the tube blank is spun, the heating device must be synchronized with the spinning wheel in the axial direction and can move independently in the radial direction of the tube blank. The specific forming process includes the following steps: S1. The tube blank is clamped on the spindle; the heating device is installed on the longitudinal slide or the spindle box and moves back and forth along the axial direction to heat the area of the tube blank to be spun to the temperature required for forming; S2. The spinning wheel performs multiple passes of alternate reciprocating shrinking and spinning of the tube blank, and after each pass of shrinking and spinning, the heating device is moved radially toward the tube blank by an optimal sensing distance, so that the temperature of the tube blank forming area is maintained in the desired temperature range; S3. After the first end of the tube blank is compressed to the required mouth size, the tube blank is turned around and clamped, so that the second end is gradually compressed into a flat bottom with a hole, and then additive manufacturing is performed on the hole to achieve bottom sealing.
2. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 1, characterized in that: The heating device is an induction coil, a flame spray gun or a laser heater; When induction heating is performed by an induction coil, the induction coil is installed on one side of the spindle box and is individually controlled by a guide rail-slider device, and is driven by a motor to move closer to or away from the barrel in the vertical direction.
3. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 2, characterized in that: When a flame spray gun is used for heating, a single-head or multi-head flame spray gun can be used according to the required temperature for heating the tube blank. The flame spray gun is installed on one side of the longitudinal slide of the machine tool and moves axially and close to the tube blank with the longitudinal slide of the machine tool, or it is installed separately on one side of the spindle box and controlled separately by a guide rail-slider device.
4. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 2, characterized in that: When a laser heater is used for heating, the laser head of the laser heater is installed on one side of the longitudinal slide of the machine tool and moves axially and approaches the tube blank with the longitudinal slide of the machine tool, or is installed separately on one side of the spindle box and is controlled separately by a guide rail-slider device.
5. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 1, characterized in that: The axial position of the heating device is located outside the rotating wheel, that is, located in the end side area of the tube blank to be formed.
6. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 1, characterized in that: During each spinning process, the moving distance of the heating device toward the tube blank should maintain the required temperature range of the material in the area to be formed of the tube blank.
7. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 1, characterized in that: The additive manufacturing includes any one of arc additive manufacturing, electron beam fuse manufacturing and laser additive manufacturing.
8. The method for integrally forming a thin-walled liner with a large diameter-to-thickness ratio by spinning and additive manufacturing according to claim 1, characterized in that: The shrinking spinning process adopts single-wheel spinning or double-wheel spinning.
Citation Information
Patent Citations
High-speed spinning sealing process method for pipe port
CN103182457A
Spin forming method of titanium alloy seamless gas cylinder
CN106077219A
Method for additive manufacturing of aluminum flange on ellipsoidal box bottom by means of electric-arc wire melting
CN110834132A
Combined necking and inward turning spinning machine
CN112828116A
Spinning forming apparatus and forming method
US20150202677A1