Preparation process of high-strength precoated sand

By adding specific components to the coated sand and adopting a specific preparation process, the strength and thermal stability of the coated sand are improved, and the problem of poor thermal stability of traditional coated sand is solved at high temperatures, which significantly improves the production of castings Efficiency and product quality.

CN118926476APending Publication Date: 2024-11-12BAIYIN HENGCHENG MASCH MFG CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411151371.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional coated sand has poor thermal stability and low strength at high temperatures, resulting in cracking of cast shells and leakage of metal liquid, affecting production efficiency and increasing waste rate.

Method used

Using high-strength coated sand preparation technology, including raw sand, silane coupling agent, alkaline phenolic resin, ethanol, urotrotropine curing agent, calcium stearate and water, through specific dissolution, stirring and mixing of sand The preparation is carried out in steps to form high-strength coated sand.

Benefits of technology

It significantly improves the tensile strength and bending strength of the coated sand at room temperature, enhances its thermal stability, reduces the cracking and leakage of the sand box, and reduces the waste rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation process of high-strength precoated sand. The precoated sand comprises the following components in parts by weight: 100 parts of crude sand; 0.05 to 0.1 part of a silane coupling agent; 1.5 to 2.5 parts of alkaline phenolic resin; 0.5 to 1.0 part of ethanol; 0.5 to 1.0 part of a urotropine curing agent; 0.15 to 0.2 part of a calcium stearate lubricant; and 1.0 to 2.0 parts of water. The preparation technology of the precoated sand comprises the following steps that alkaline phenolic resin is dissolved in ethyl alcohol, and an alkaline phenolic resin solution is formed; preparing urotropine into an aqueous solution; raw sand is preheated and stirred, then an alkaline phenolic resin solution is added for sand mixing, then a urotropine aqueous solution is added for sand mixing, then a silane coupling agent is added for sand mixing for 50 s, finally calcium stearate is added for sand mixing for about 50 s, sand discharging is conducted, and the precoated sand is obtained. The precoated sand disclosed by the invention has high strength, is simple in preparation process and is most suitable for being applied to production of a shell mold casting process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting, and in particular relates to a process for preparing high-strength coated sand. Background Art

[0002] When the coated sand prepared by traditional technology is used to cast grinding balls in the shell casting process, it has poor thermal stability and low strength at high temperatures, which makes it unable to resist the thermal stress caused by the expansion of the sand core and the pressure of the molten steel itself during the casting process. It often causes the sand box composed of the shell mold to crack, and a large amount of metal liquid leaks, causing the grinding balls to be scrapped. At the same time, leakage in small parts can easily cause sand sticking or steel ball adhesion. This affects the cleaning work of the casting surface and even causes the grinding balls to be scrapped, reducing production efficiency and increasing scrap rate. In order to serve the shell mold process production of small diameter grinding balls, attempts are made to improve the coated sand preparation process. Summary of the invention

[0003] The purpose of the present invention is to provide a high-strength coated sand preparation process to solve the problems raised in the above background technology.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A high-strength coated sand, the coated sand comprising the following components by weight:

[0006] 100 parts of raw sand;

[0007] Silane coupling agent 0.05-0.1 part;

[0008] 1.5-2.5 parts of alkaline phenolic resin;

[0009] Ethanol 0.5-1.0 parts;

[0010] 0.5-1.0 part of hexamethylenetetramine curing agent;

[0011] Calcium stearate lubricant 0.15-0.2 parts;

[0012] 1.0-2.0 parts of water.

[0013] The raw sand specification is 70 / 100 desert sand.

[0014] A high-strength coated sand preparation process comprises the following steps:

[0015] 1) dissolving alkaline phenolic resin in ethanol to form an alkaline phenolic resin solution;

[0016] 2) preparing an aqueous solution of urotropine;

[0017] 3) Preheat the raw sand to 125±5°C, stir for 75±5s, then add the alkaline phenolic resin solution in step 1) and mix the sand for about 10s, the sand temperature is about 100°C, then add the urotropine aqueous solution in step 2) and mix the sand for about 10s, the sand temperature is 80±5°C, add the silane coupling agent and mix the sand for 50s, add calcium stearate and mix the sand for about 50s, the sand temperature is about 60°C, and the coated sand is obtained.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention adopts a treatment process combining stable solidification and rolling and sintering, with a simple process route. At the same time, waterproof and anti-corrosion primers and coatings are sprayed on the prepared fly ash blanks, which can effectively realize the harmless utilization and treatment of hazardous waste fly ash, effectively avoid secondary pollution, and reduce environmental pressure. DETAILED DESCRIPTION

[0020] The present invention will be described in detail below in conjunction with specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0021] A high-strength coated sand, the coated sand comprising the following components by weight:

[0022] 100 parts of raw sand;

[0023] Silane coupling agent 0.05-0.1 part;

[0024] 1.5-2.5 parts of alkaline phenolic resin;

[0025] Ethanol 0.5-1.0 parts;

[0026] 0.5-1.0 part of hexamethylenetetramine curing agent;

[0027] Calcium stearate lubricant 0.15-0.2 parts;

[0028] 1.0-2.0 parts of water.

[0029] The raw sand specification is 70 / 100 desert sand.

[0030] A high-strength coated sand preparation process comprises the following steps:

[0031] 1) dissolving alkaline phenolic resin in ethanol to form an alkaline phenolic resin solution;

[0032] 2) preparing an aqueous solution of urotropine;

[0033] 3) Preheat the raw sand to 125±5°C, stir for 75±5s, then add the alkaline phenolic resin solution in step 1) and mix the sand for about 10s, the sand temperature is about 100°C, then add the urotropine aqueous solution in step 2) and mix the sand for about 10s, the sand temperature is 80±5°C, add the silane coupling agent and mix the sand for 50s, add calcium stearate and mix the sand for about 50s, the sand temperature is about 60°C, and the coated sand is obtained.

[0034] Example 1

[0035] 0.5 kg of ethanol was dissolved in 1.7 kg of alkaline phenolic resin to obtain an alkaline phenolic resin solution, and 0.5 kg of urotropine was dissolved in 1.5 kg of water to obtain a urotropine aqueous solution.

[0036] First, add 100kg of raw sand (70 / 100 mesh desert sand) into the mixer, heat to 125±5℃, and stir for 75±5S. Add alkaline phenolic resin solution, stir for 10S, and the sand temperature is about 100℃. Add urotropine aqueous solution, stir for about 10S, and the sand temperature is 80±5℃. Add 0.05kg of silane coupling agent, mix the sand for 50S, add 0.16kg of calcium stearate, stir for about 50S, and the sand temperature is 60℃, then sand out.

[0037] The coated sand produced in this example has a room temperature tensile strength of 3.3MPa and a room temperature flexural strength of 7.3MPa. The ordinary coated sand produced by the traditional thermal method has a room temperature tensile strength of 2.43MPa and a room temperature flexural strength of 4.5MPa. The room temperature strength is increased by 35%, and the room temperature flexural strength is increased by 62%.

[0038] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention.

Claims

1. A high-strength coated sand, characterized in that: The coated sand comprises the following components by weight: 100 parts of raw sand; Silane coupling agent 0.05-0.1 part; 1.5-2.5 parts of alkaline phenolic resin; Ethanol 0.5-1.0 parts; 0.5-1.0 part of hexamethylenetetramine curing agent; Calcium stearate lubricant 0.15-0.2 parts; 1.0-2.0 parts of water.

2. The high-strength coated sand according to claim 1, characterized in that: The raw sand specification is 70 / 100 desert sand.

3. The process for preparing high-strength coated sand according to claim 1, characterized in that: The steps include: 1) dissolving alkaline phenolic resin in ethanol to form an alkaline phenolic resin solution; 2) preparing an aqueous solution of urotropine; 3) Preheat the raw sand to 125±5°C, stir for 75±5s, then add the alkaline phenolic resin solution in step 1) and mix the sand for about 10s, the sand temperature is about 100°C, then add the urotropine aqueous solution in step 2) and mix the sand for about 10s, the sand temperature is 80±5°C, add the silane coupling agent and mix the sand for 50s, add calcium stearate and mix the sand for about 50s, the sand temperature is about 60°C, and the coated sand is obtained.

Citation Information

Cited By

  • Preparation method of high-temperature-resistant low-expansion precoated sand

    CN119794257A