Sand box and casting process applying same

By setting up a support frame and base in the sand box and using casting sand mixed with magnesium oxide and phosphate, the problem of molded sand cracks caused by bending of steel bars is solved, the casting quality and support effect of castings are improved, and effective for castings in complex shapes is achieved. Support and high-quality casting.

CN118926489AActive Publication Date: 2024-11-12WUXI LINGTONG CASTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410981202.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

In the prior art, the bending of the steel bar will cause cracks in the molding sand, affecting the casting quality of the casting, and cannot effectively support the molding sand of the castings with complex shapes, resulting in a decrease in the casting quality.

Method used

Design a sand box, by setting a support frame and base in the box, determining the reference surface according to the shape of the casting, dividing the space, casting using casting sand mixed with magnesium oxide and phosphate, and controlling the medium temperature and the management of inflow and outflow pipes , ensure the stability and support effect of cast sand.

Benefits of technology

The cracks and collapses of casting sand are avoided, the casting quality of castings is improved, the installation accuracy of the support frame and the structural strength of casting sand are ensured, the deformation and cracks of castings are reduced, and the overall quality of casting is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926489A_ABST
    Figure CN118926489A_ABST
Patent Text Reader

Abstract

The invention relates to a sand box and a casting process applying the sand box. The sand box comprises a box body; the base is arranged in the box body; the supporting frame is arranged on the base; the foundry sand is arranged in the box body and covers the base and the supporting frame; wherein the inner reference surface of the box body is determined according to the shape of the casting, and the inner space of the box body is divided according to the reference surface; the position of the support frame arranged on the base is positioned on the reference surface in the box body; the support frame is positioned in the inner space of each box body; a channel is formed in the base and the supporting frame. The box body is provided with an inlet and outlet pipe through which a medium flows in and out; and the inlet and outlet pipe is communicated with the channel. The problems that in an existing scheme, after a steel bar is bent, the steel bar can deform to drive molding sand to generate cracks, the casting quality of a casting is influenced, the position, close to a cavity, of the molding sand cannot be effectively supported, the molding sand can deform to generate cracks, and the casting quality of the casting is influenced are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of casting, in particular to a sand box and a casting process using the sand box. Background Art

[0002] For castings with complex shapes and complex cavity surfaces, a steel skeleton is often embedded in the sand to prevent the sand from collapsing. The steel bars are bent and cut as needed, and then several steel bars are welded into an integral steel skeleton.

[0003] The structural strength of steel bars is low. After being bent, the steel bars will deform and cause cracks in the molding sand, affecting the casting quality. At the same time, steel bars can improve the overall structural strength of the molding sand, but for castings with complex shapes, the molding sand cannot form effective support near the mold cavity, and the molding sand will deform and crack, affecting the casting quality.

[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0005] In view of the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a sand box and a casting process using the sand box, so as to solve the problems in the prior art that after the steel bars are bent, the steel bars will be deformed, causing the molding sand to crack, thereby affecting the casting quality of the casting; and the molding sand cannot form effective support near the mold cavity, and the molding sand will be deformed and cracked, thereby affecting the casting quality of the casting.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A sand box;

[0008] A box body; a base, arranged in the box body; a support frame, arranged on the base; casting sand, placed in the box body and covering the base and the support frame; wherein the reference surface in the box body is determined according to the shape of the casting, and the space in the box body is divided according to the reference surface; the support frame is arranged at a position on the base located on the reference surface in the box body; the support frame is located in each space in the box body; a channel is formed in the base and the support frame; inlet and outlet pipes for flowing in and out of the medium are arranged on the box body; the inlet and outlet pipes are connected to the channel.

[0009] A further technical solution is that the base includes: a bottom block, which is arranged in the middle position of the box body; and a reference plate, which is radially arranged around the bottom block; wherein the upper surface of the bottom block and the upper surface of the reference plate are located on the reference plane inside the box body.

[0010] A further technical solution is that the support frame includes: a main frame, which is arranged on the reference plate; a sub-frame, which is arranged on the main frame; and an extension portion, which is arranged in parallel on the sub-frame; wherein the sub-frame extends straight along the casting; and the extension portion is parallel to the casting surface.

[0011] A further technical solution is that the foundry sand includes magnesium oxide, phosphate and raw sand; the ratio of magnesium oxide to phosphate is 2.3; and the total mass of magnesium oxide and phosphate accounts for 8% of the mass of the raw sand.

[0012] A further technical solution is that a valve and a detection device are arranged on the inlet and outlet pipes; the valve opens and closes the inlet and outlet pipes; and the detection end of the detection device extends into the inlet and outlet pipes to detect the pressure inside the inlet and outlet pipes.

[0013] A casting process using a sand box comprises the following steps:

[0014] Analysis steps: Modeling and analyzing the casting to obtain modeling data, and determining the data of the reference surface in the box according to the modeling data; establishing the initial data of the support frame according to the modeling data on the reference surface data; simulating the modeling data, dividing the data of the space in the box on the reference surface data according to the initial data of the support frame, and obtaining the final data of the support frame;

[0015] Preparation steps: according to the modeling data, make a mold and trim the mold; according to the reference surface data, make a base; according to the final data of the support frame, make a support frame;

[0016] Sand mold steps: install the base in the box according to the reference surface data; install the mold on the base; install the support frame on the base according to the final data of the support frame;

[0017] Steps of closing the box: adding the foundry sand into the box in multiple times and in a quantitative manner; during each adding process: spreading the foundry sand flat, and then pressing the foundry sand flat; closing the box and tightening it;

[0018] Casting steps: pouring casting medium into the mold cavity and then cooling; during the casting process, hot medium flows into the channel; during the cooling process of the casting, normal temperature medium flows into the channel;

[0019] Unpacking steps: Cool the casting to 300℃, unpack, clean the sand and partially cut the runner and riser;

[0020] First heat treatment step: the casting is locally heated to 750°C, with a heating rate of 95-105°C; gradually placed in an insulation box for 2.5 hours;

[0021] The second heat treatment step specifically includes:

[0022] The first heating process: the casting is heated to 1010℃~1030℃, and the heating rate is 195~205℃; the heat preservation time is 1.5h; then air-cooled to room temperature; the remaining parts of the runner and riser are cut, and the positions of the runner and riser of the casting are polished;

[0023] The second heating process: the casting is heated to 580℃~585℃, the heating rate is 140~145℃; the holding time is 1.5h; then the casting is cooled to 200℃ in the furnace and taken out of the furnace.

[0024] A further technical solution is that the analysis step further includes a simulation step: simulating the casting and cooling of the casting according to the modeling data to obtain the temperature data of the sand mold cavity during the casting process, T1; obtaining the temperature data of the sand mold cavity during the cooling process of the casting, T2;

[0025] The casting steps include: pouring a casting medium into the mold cavity and then cooling it; during the casting process of the casting, a hot medium flows into the channel; according to the temperature data T1 in the sand mold cavity, the temperature of the hot medium and the interval time of the introduction are adjusted; during the cooling process of the casting, a normal temperature medium flows into the channel, and according to the temperature data T2 in the sand mold cavity, the flow rate and the interval time of the normal temperature medium are adjusted.

[0026] A further technical solution is that the sand molding step also includes a sand mixing step: magnesium oxide and phosphate solution are mixed in a ratio of 2.3:1 to form a mixture, and the mixture is added into the raw sand for stirring, and the mass of the mixture accounts for 8% of the mass of the raw sand.

[0027] Compared with the prior art, the beneficial technical effects of the present invention are as follows: (1) The position of the support frame arranged on the base is located on the reference plane in the box body; the support frame is located in the space in each box body, and the support frames in each space are not connected, so that the support frames do not affect each other, the support frames do not deform, and the casting sand does not crack; at the same time, the support frames are installed on the same reference plane, which improves the installation accuracy of the support frames and avoids affecting the casting quality of the casting;

[0028] The foundry sand covers the base and the support frame, and the support frame supports the foundry sand to prevent the foundry sand from collapsing and cracking, which would affect the casting of the casting.

[0029] (2) The extension parts can be arranged in parallel on one side of the branch section, the extension parts can be arranged in parallel on both sides of the branch section, or the extension parts can be arranged alternately on both sides of the branch section; the shape of the extension parts can be determined according to the surface shape of the casting;

[0030] After the foundry sand fills the box, the foundry sand covers the base and the support frame, and the support frame plays a structural support role for the foundry sand, thereby preventing the foundry sand from collapsing and affecting the casting of the casting.

[0031] (3) When the sand box is closed, the sand box is inverted, and the casting sand can self-harden at room temperature, thereby improving the structural strength of the casting sand itself. The self-hardened casting sand plays a structural supporting role for the base and the support frame; the support frame and the casting sand support each other to prevent the casting sand from collapsing and affecting the casting of the casting.

[0032] (4) The foundry sand is flattened layer by layer, and the thickness of the flattened foundry sand is relatively thin, so that the foundry sand is compacted. After the foundry sand is hardened, the density of the foundry sand is relatively high, and the foundry sand can form a stable support for the support frame;

[0033] The foundry sand is added into the box in quantitative amounts for multiple times. The foundry sand cannot completely submerge the base and the support frame. When the foundry sand is pressed down, the downward pressure acting on the support frame is small and will not cause deformation of the support frame.

[0034] (5) The runner and riser are not completely cut during the unpacking process. After the first heating process, the grains of the casting are refined and the carbide distribution is uniform. At the same time, the stress of the casting is eliminated after the first heating process, and the stress of the runner and riser is also eliminated, which makes it convenient to cut and grind the remaining parts of the runner and riser, avoiding cracks during cutting and grinding. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The figure shows a schematic structural diagram of a sand box according to the first embodiment of the present invention.

[0036] Figure 2 A schematic diagram of the top structure of the base according to the first embodiment of the present invention is shown.

[0037] Figure 3 A schematic structural diagram of a support frame according to a first embodiment of the present invention is shown.

[0038] Markings in the accompanying drawings: 1. box body; 11. inlet and outlet pipes; 12. second slot; 13. valve; 14. detection device; 2. base; 21. bottom block; 22. reference plate; 23. first slot; 24. plate; 25. notch; 3. support frame; 31. main frame; 32. auxiliary frame; 321. sleeve; 322. branch section; 33. extension; 4. casting sand; 5. channel. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the present invention clearer, the device proposed by the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will be clearer. It should be noted that the accompanying drawings adopt a very simplified form and use non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, please refer to the accompanying drawings. It should be noted that the structure, proportion, size, etc. illustrated by the accompanying drawings of this specification are only used to match the content disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no technical substantive significance. Any modification of the structure, change of the proportional relationship or adjustment of the size, without affecting the effect that the present invention can produce and the purpose that can be achieved, should still fall within the scope of the technical content disclosed by the present invention.

[0040] First embodiment:

[0041] Figure 1 The figure shows a schematic structural diagram of a sand box according to the first embodiment of the present invention. Figure 2 A schematic diagram of the top structure of the base according to the first embodiment of the present invention is shown. Figure 3 FIG. 1 is a schematic diagram showing the structure of the support frame according to the first embodiment of the present invention. Figure 1-Figure 3 As shown, the present invention discloses a sand box.

[0042] The sand box comprises: casting sand 4, a box body 1, a base 2 arranged at the lower end of the box body 1, and a support frame 3 arranged on the base 2.

[0043] The casting sand 4 is placed in the box 1 and covers the base 2 and the support frame 3. The reference surface in the box 1 is determined according to the shape of the casting, and the space in the box 1 is divided according to the reference surface.

[0044] The support frame 3 is arranged at the position of the base 2 on the reference surface in the box 1. The support frame 3 is located in the space in each box 1, and the support frames 3 in each space are not connected, so that the support frames 3 do not affect each other, the support frames 3 do not deform, and the casting sand 4 does not crack. At the same time, each support frame 3 is installed on the same reference surface, which improves the installation accuracy of the support frame 3 and avoids affecting the casting quality of the casting.

[0045] The casting sand 4 covers the base 2 and the support frame 3, and the support frame 3 supports the casting sand 4 to prevent the casting sand 4 from collapsing and cracking, which would affect the casting of the casting.

[0046] A channel 5 is formed in the base 2 and the support frame 3. An inlet and outlet pipe 11 for the medium to flow in and out is arranged on the box body 1. The inlet and outlet pipe 11 is connected to the channel 5.

[0047] During the casting process, hot medium flows into the channel 5 to keep the mold cavity warm, thereby preventing the casting medium from contacting the casting sand 4 during casting and preventing the casting medium from shrinking due to cooling.

[0048] During the cooling process of the casting medium, the temperature should be prevented from dropping too fast. A medium at room temperature is introduced into the channel 5 so that the temperature of the casting medium drops slowly and gradually solidifies to form a casting.

[0049] The base 2 includes: a bottom block 21 arranged at a middle position in the box body 1 and a reference plate 22 arranged radially around the bottom block 21 .

[0050] The upper surface of the bottom block 21 and the upper surface of the reference plate 22 are located on the reference surface inside the box body 1 .

[0051] Exemplarily, the cross section of the bottom block 21 is a polygon. First slots 23 are formed in parallel around the bottom block 21. Second slots 12 are formed in parallel around the inner surface of the box body 1. One end of the reference plate 22 is inserted into the first slot 23, and the channel 5 of the reference plate 22 is connected to the channel 5 of the bottom block 21. The other end of the reference plate 22 is inserted into the second slot 12.

[0052] The bottom block 21 and the box body 1 restrict the two ends of the reference plate 22 so that the upper surface of the bottom block 21 and the upper surface of the reference plate 22 can form an accurate reference surface.

[0053] A plate 24 is provided at one end of the reference plate 22. A notch 25 is formed on the bottom block 21, and the notch 25 is connected to the first slot 23. When one end of the reference plate 22 is inserted into the first slot 23, the plate 24 is placed in the notch 25. The reference plate 22 is fixedly connected to the bottom block 21 by bolts. After the bolt passes through the plate 24, the thread is screwed into the notch 25.

[0054] When the medium flows along the channel 5 of the reference plate 22 and the channel 5 of the bottom block 21 , no leakage occurs between the reference plate 22 and the bottom block 21 .

[0055] The support frame 3 includes: a main frame 31 vertically arranged on the reference plate 22, a sub-frame 32 arranged on the main frame 31, and an extension 33 arranged in parallel on the sub-frame 32. The sub-frame 32 extends along the casting straight line. The extension 33 is parallel to the casting surface.

[0056] The lower end of the main frame 31 is threadedly connected to the reference plate 22. The inner channel 5 of the reference plate 22 extends upward to communicate with the inner channel 5 of the main frame 31.

[0057] The sub-frame 32 includes a sleeve 321 sleeved on the main frame 31 and a branch section 322 extending along the straight line of the casting. The branch section 322 is connected to the sleeve 321. The sleeve 321 is fixed to the main frame 31 by bolts. The bolts pass through the sleeve 321 and are screwed into the main frame 31.

[0058] For example, the number of the branch section 322 can be single or multiple. The number of the branch section 322 is determined according to the surface condition of the casting. When the surface of the casting is flat, the number of the branch section 322 is single. When the shape of the surface of the casting changes, the number of the branch section 322 is multiple.

[0059] Exemplarily, the extension part 33 may be arranged in parallel on one side of the branch section 322, the extension part 33 may be arranged in parallel on both sides of the branch section 322, or the extension part 33 may be arranged alternately on both sides of the branch section 322. The shape of the extension part 33 may be determined according to the surface shape of the casting.

[0060] After the foundry sand 4 fills the box 1, the foundry sand 4 covers the base 2 and the support frame 3, and the support frame 3 plays a structural support role for the foundry sand 4, so as to prevent the foundry sand 4 from collapsing and affecting the casting of the casting.

[0061] The foundry sand 4 comprises magnesium oxide, phosphate and raw sand. The magnesium oxide / phosphate ratio is 2.3. The total mass of magnesium oxide and phosphate accounts for 8% of the mass of the raw sand.

[0062] When the sand box is closed, the sand box is inverted, and the casting sand 4 can be self-hardened at room temperature to improve the structural strength of the casting sand 4. The self-hardened casting sand 4 plays a structural support role for the base 2 and the support frame 3. The support frame 3 and the casting sand 4 support each other to prevent the casting sand 4 from collapsing and affecting the casting of the casting.

[0063] A valve 13 and a detection device 14 are provided on the inlet and outlet pipe 11. The valve 13 opens and closes the inlet and outlet pipe 11. The detection end of the detection device 14 extends into the inlet and outlet pipe 11 to detect the pressure in the inlet and outlet pipe 11.

[0064] The valve 13 is used to open and close the inlet and outlet pipes 11 to control the interval time of the heat medium and the normal temperature medium. Exemplarily, the detection device 14 is a pressure sensor. The detection device 14 detects the pressure in the inlet and outlet pipes 11, thereby controlling the amount of heat medium and the normal temperature medium in the channel 5.

[0065] Second embodiment:

[0066] A casting process using a sand box comprises the following steps:

[0067] Analysis steps: Modeling and analyzing the casting to obtain modeling data, and determining the data of the reference surface in the box 1 according to the modeling data. Establishing the initial data of the support frame 3 according to the modeling data on the reference surface data. Simulating the modeling data, dividing the data of the space in the box 1 on the reference surface data according to the initial data of the support frame 3, and obtaining the final data of the support frame 3.

[0068] In the analysis step, modeling analysis is performed according to the size of the casting to obtain modeling data. According to the modeling data, the data of the reference surface in the box body 1 are determined. On the reference surface data, the initial data of the support frame 3 is established according to the modeling data.

[0069] The initial data of the support frame 3 includes the complete size data of the support frame 3. When the support frame 3 is a whole, any position of the support frame 3 is subjected to force, which will affect the position of the support frame 3. By dividing the space in the box 1, the support frame 3 is divided into several structures, and the support frames 3 in different spaces do not interfere with each other and will not affect each other.

[0070] The surface shape of the casting is obtained according to the modeling data. When the surface of the casting is flat, the space division is large. When the surface shape of the casting changes, the space division is small. After the space division, the final data of the support frame 3 is obtained according to the data of the space in the box 1.

[0071] The analysis step also includes a simulation step: simulating the casting and cooling of the casting according to the modeling data to obtain the temperature data in the sand mold cavity during the casting process, T1, and the temperature data in the sand mold cavity during the cooling process of the casting, T2.

[0072] The casting medium is poured into the mold cavity, and the temperature in the mold cavity rises rapidly. After the casting is completed, the casting medium cools down, the temperature of the casting in the mold cavity drops, and the casting medium solidifies to form a casting. By simulating the above situation, the temperature data T1 and T2 are recorded.

[0073] Preparation steps: According to the modeling data, a mold is made and the mold is trimmed. According to the reference surface data, a base 2 is made. According to the final data of the support frame 3, a support frame 3 is made.

[0074] The mold is trimmed to ensure that the mold surface is smooth. When the base 2 is installed in the box 1, the upper surface of the bottom block 21 and the upper surface of the reference plate 22 and the reference surface are located in the same plane. According to the final data of the support frame 3, the support frame 3 is manufactured so that the sub-frame 32 extends along the straight line of the casting and the extension part 33 is parallel to the surface of the casting.

[0075] Sand mold step: install the base 2 in the box 1 according to the reference surface data. Install the mold on the base 2. Specifically, the mold is installed on the upper surface of the bottom block 21. Install the support frame 3 on the base 2 according to the final data of the support frame 3, ensuring the position of the main frame 31 installed on the reference plate 22, the position of the sub-frame 32 installed on the main frame 31, the position of the extension 33 set on the sub-frame 32 and the shape of the extension 33.

[0076] The sand molding step also includes the sand mixing step:

[0077] The magnesium oxide and the phosphate solution are mixed in a ratio of 2.3:1 to form a mixture, and the mixture is added into the raw sand for stirring, and the mass of the mixture accounts for 8% of the mass of the raw sand.

[0078] Steps of closing the box: the foundry sand 4 is quantitatively added into the box body 1 in multiple times. During each adding process: the foundry sand 4 is spread flat, and then the foundry sand 4 is flattened. The box is closed and tightened.

[0079] The casting sand 4 is added into the box 1, and after the casting sand 4 is laid flat, the casting sand 4 is flattened. The above steps are repeated, and the casting sand 4 is flattened layer by layer. The casting sand 4 at the bottom gradually hardens. After the casting sand 4 in the box 1 is completely hardened, the casting sand 4 supports the base 2 and the support frame 3. At the same time, the support frame 3 forms an internal support for the casting sand 4 to prevent the casting sand 4 from breaking and falling off.

[0080] The casting sand 4 is flattened layer by layer, and the flattened thickness of a single casting sand 4 is relatively thin, so that the single casting sand 4 is compacted. After the casting sand 4 hardens, the density of the casting sand 4 is relatively high, and the casting sand 4 can form a stable support for the support frame 3.

[0081] If all the foundry sand 4 is injected into the box body 1, the foundry sand 4 will submerge the base 2 and the support frame 3. At this time, the foundry sand 4 is pressed downward, and the downward pressure will act on the support frame 3, causing the support frame 3 to deform.

[0082] The foundry sand 4 is quantitatively added into the box body 1 for multiple times. The foundry sand 4 cannot completely submerge the base 2 and the support frame 3. When the foundry sand 4 is pressed down, the downward pressure acting on the support frame 3 is small and will not cause deformation of the support frame 3.

[0083] Casting steps: Pour the casting medium into the mold cavity and then cool it. During the casting process, hot medium flows into the channel 5. During the cooling process of the casting, the channel 5 flows into the medium of normal temperature.

[0084] The casting step includes: pouring the casting medium into the mold cavity and then cooling. During the casting process, the hot medium flows into the channel 5. According to the temperature data T1 in the sand mold cavity, the temperature of the hot medium and the interval time of the introduction are adjusted. During the cooling process of the casting, the normal temperature medium flows into the channel 5, and according to the temperature data T2 in the sand mold cavity, the flow rate and the interval time of the normal temperature medium are adjusted.

[0085] The heat medium is introduced into the channel 5 by introducing a certain amount of heat medium. When a certain pressure is reached in the channel 5, the heat medium is stopped from being introduced into the channel 5. After stopping for a period of time, the heat medium is discharged, and a certain amount of heat medium is introduced again, and the above steps are repeated.

[0086] By introducing a fixed amount of heat medium at a time, the heat medium is dispersed in the channel 5, and the cavity is evenly heated. If the heat medium is continuously introduced and discharged, the heat medium is discharged before it is completely distributed in the channel 5, and the cavity cannot be evenly heated.

[0087] Before the casting medium is poured into the mold cavity, the mold cavity needs to be heated. During the process of pouring the casting medium into the mold cavity, the mold cavity needs to be kept warm. This avoids excessive temperature difference between the inside and outside of the casting medium and ensures the quality of the casting after casting.

[0088] The temperature of the heat medium flowing into the channel 5 before the casting medium is poured into the mold cavity is greater than the temperature of the heat medium flowing into the channel 5 during the casting medium is poured into the mold cavity. The interval time of the heat medium flowing into the channel 5 before the casting medium is poured into the mold cavity is less than the interval time of the heat medium flowing into the channel 5 during the casting medium is poured into the mold cavity.

[0089] Before the casting medium is poured into the cavity, the high-frequency and high-temperature hot medium flows into the channel 5, causing the temperature in the cavity to rise rapidly. After the casting medium is poured into the cavity, the temperature of the casting medium itself ensures that the temperature in the cavity does not drop rapidly. Before the casting medium is poured, the cavity needs to be insulated to avoid the temperature in the cavity from losing too quickly and to avoid a large temperature difference between the inside and outside of the casting medium.

[0090] During the process of pouring the casting medium into the mold cavity, the temperature and frequency of the hot medium flowing into the mold cavity decrease accordingly, which plays a certain role in heat preservation.

[0091] During the cooling process of the casting, a normal temperature medium flows into the channel 5. According to the temperature data T2 in the sand mold cavity, the flow rate, number of injection intervals and injection interval time of the normal temperature medium are adjusted.

[0092] The normal temperature medium is introduced into the channel 5 by introducing a certain amount of the normal temperature medium, and when a certain pressure is reached in the channel 5, the normal temperature medium is stopped from being introduced into the channel 5. After stopping for a period of time, the normal temperature medium is discharged, and a certain amount of the normal temperature medium is introduced again, and the above steps are repeated.

[0093] The heat of the casting medium is transferred to the support frame 3 through the casting sand 4, and then transferred to the channel 5. By introducing a certain amount of normal temperature medium at a time, the normal temperature medium is dispersed in the channel 5, and the normal temperature medium is discharged after being heated, so that the cavity can be cooled evenly. If the normal temperature medium is continuously introduced and continuously discharged, the normal temperature medium is discharged before it is completely distributed in the channel 5, and the heat in the channel 5 cannot be completely discharged, and the heat in the cavity drops unevenly, affecting the quality of the casting.

[0094] After the casting medium is poured into the mold cavity, the mold cavity needs to be cooled down. The mold cavity is cooled down slowly to avoid excessive temperature difference between the inside and outside of the casting medium, thus ensuring the quality of the casting after casting.

[0095] As the temperature in the mold cavity drops, the temperature data T2 in the sand mold cavity gradually decreases. The lower the temperature data T2 in the sand mold cavity, the faster the flow rate of the normal temperature medium and the longer the interval time for the normal temperature medium to pass through.

[0096] When the temperature in the mold cavity just starts to drop, the temperature in the sand mold cavity is relatively high, and more heat is transferred to the channel 5. The flow rate of the normal temperature medium is relatively slow, and the normal temperature medium gradually fills the channel 5. During the process, the temperature of the normal temperature medium in the channel 5 gradually rises, and the process of the normal temperature medium absorbing heat is relatively gentle, which prevents the casting medium from cooling down too quickly and affecting the temperature difference between the inside and outside of the casting medium. At the same time, the normal temperature medium is introduced at a short interval. Due to the high temperature in the sand mold cavity, the normal temperature medium in the channel 5 heats up quickly, and the normal temperature medium is introduced at a shorter interval, so that the normal temperature medium is introduced into the channel 5 at a high frequency, completing the continuous cooling of the sand mold cavity.

[0097] The cooling time in the mold cavity gradually increases, the temperature in the sand mold cavity gradually decreases, the heat transferred to the channel 5 begins to decrease, and the flow rate of the normal temperature medium is faster, so that the normal temperature medium can quickly fill the channel 5. At the same time, the normal temperature medium is introduced for a long time. Due to the low temperature in the sand mold cavity, the normal temperature medium in the channel 5 heats up slowly. By extending the normal temperature medium introduction interval, the normal temperature medium in the channel 5 is discharged after heating to a certain degree.

[0098] Before casting, hot medium flows into the channel 5 to preheat the cavity in advance, thus avoiding direct baking of the cavity and causing cracks on the cavity surface.

[0099] Unpacking steps: unpack the casting after it cools to 300℃, remove sand and partially cut the runner and riser.

[0100] After unpacking, most of the runners and risers are cut, leaving the runners and risers close to the casting.

[0101] First heat treatment step: The casting is locally heated to 750°C, with a heating rate of 95-105°C. It is gradually placed in an incubator for 2.5 hours;

[0102] According to the modeling data, the local position of the casting is determined. The local position of the casting is the thicker position of the casting. Due to the irregular shape of the casting, the thickness of different positions of the casting is different. If the casting adopts a uniform heating time, the thinner position of the casting is fully heated, and the thicker position of the casting is not fully heated.

[0103] In the first heat treatment step, the casting is locally heated to create a certain temperature difference at different locations of the casting. During the local heating of the casting, the heating rate is slow to prevent the local heating of the casting from being too fast. During the local heating of the casting, the heat from the heated location of the casting is transferred to the non-heated location of the casting. After a certain period of heat preservation, the temperature of the thicker location of the casting is consistent inside and outside, and the temperature of the thinner location of the casting rises to a certain extent. The temperature of the thicker location of the casting is greater than the temperature of the thinner location of the casting.

[0104] The second heat treatment step specifically includes:

[0105] First heating process: The casting is heated to 1010℃~1030℃, and the heating rate is 195~205℃. Keep warm for 1.5h. Then air cool to room temperature. Cut the remaining part of the runner and riser, and grind the casting runner and riser position.

[0106] Second heating process: The casting is heated to 580℃~585℃, and the heating rate is 140~145℃. The holding time is 1.5h. Then the casting is cooled to 200℃ and taken out of the furnace.

[0107] Since the casting has been heated, a faster heating rate is used during the first heating process, so that the casting can be quickly heated to 1010℃~1030℃. Since the temperature difference inside and outside the thicker part of the casting is consistent, the first heating process only requires a shorter holding time.

[0108] The runners and risers are not completely cut during the unpacking process. After the first heating process, the casting grains are refined and the carbide distribution is uniform. At the same time, the stress of the casting is eliminated after the first heating process, and the stress of the runners and risers is also eliminated, which makes it easier to cut and grind the remaining parts of the runners and risers to avoid cracks during cutting and grinding.

[0109] Since the runner and riser are kept close to the casting, the heat generated during the cutting process will not be transferred to the casting. At the same time, the cutting and grinding margins of the remaining parts of the runner and riser are small, and the heat generated has less impact on the casting.

[0110] The hardness of the casting is increased through the second heating process and has reached the use requirements of the casting.

[0111] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0112] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A sand box, characterized in that: include: Box body (1); A base (2) is arranged inside the box (1); A support frame (3) is arranged on the base (2); Foundry sand (4), placed in the box (1) and covering the base (2) and the support frame (3); The reference plane inside the box (1) is determined according to the shape of the casting, and the space inside the box (1) is divided according to the reference plane; the support frame (3) is arranged on the base (2) at a position located on the reference plane inside the box (1); the support frame (3) is located in the space inside each box (1); a channel (5) is formed inside the base (2) and the support frame (3); an inlet and outlet pipe (11) for the inflow and outflow of the medium is arranged on the box (1); the inlet and outlet pipe (11) is connected to the channel (5).

2. The flask according to claim 1, characterized in that: The base (2) comprises: A bottom block (21) is arranged at a middle position in the box body (1); A reference plate (22) is radially arranged around the bottom block (21); Wherein, the upper surface of the bottom block (21) and the upper surface of the reference plate (22) are located on the reference surface inside the box body (1).

3. The flask according to claim 2, characterized in that: The support frame (3) comprises: A main frame (31) is arranged on the reference plate (22); A sub-frame (32) is arranged on the main frame (31); An extension portion (33) is arranged in parallel on the sub-frame (32); The sub-frame (32) extends in a straight line along the casting; and the extension portion (33) is parallel to the surface of the casting.

4. The flask according to claim 1, characterized in that: The foundry sand (4) comprises magnesium oxide, phosphate and raw sand; the ratio of magnesium oxide to phosphate is 2.3; the total mass of magnesium oxide and phosphate accounts for 8% of the mass of the raw sand.

5. The flask according to claim 1, characterized in that: The inlet and outlet pipe (11) is provided with a valve (13) and a detection device (14); the valve (13) opens and closes the inlet and outlet pipe (11); the detection end of the detection device (14) extends into the inlet and outlet pipe (11) to detect the pressure in the inlet and outlet pipe (11).

6. A casting process using a sand box, using the sand box as claimed in claim 1; characterized in that: The steps include: Analysis steps: modeling and analyzing the casting to obtain modeling data, determining the data of the reference surface inside the box (1) according to the modeling data; establishing the initial data of the support frame (3) on the reference surface data according to the modeling data; Simulating modeling data, dividing the data of the space inside the box (1) on the reference surface data according to the initial data of the support frame (3), and obtaining the final data of the support frame (3); Preparation steps: according to the modeling data, a mold is made, and the mold is trimmed; according to the reference surface data, a base (2) is made; according to the final data of the support frame (3), a support frame (3) is made; Sand mold step: install the base (2) in the box (1) according to the reference surface data; install the mold on the base (2); install the support frame (3) on the base (2) according to the final data of the support frame (3); box closing step: add the casting sand (4) into the box (1) in a quantitative manner for multiple times; during each adding process: spread the casting sand (4) flat, and then flatten the casting sand (4); close the box and tighten; Casting steps: pouring a casting medium into the mold cavity and then cooling it; during the casting process, a hot medium flows into the channel (5); during the cooling process of the casting, a normal temperature medium flows into the channel (5); Unpacking steps: Cool the casting to 300℃, unpack, clean the sand and partially cut the runner and riser; First heat treatment step: the casting is locally heated to 750°C, with a heating rate of 95-105°C; gradually placed in an insulation box for 2.5 hours; The second heat treatment step specifically includes: The first heating process: the casting is heated to 1010℃~1030℃, and the heating rate is 195~205℃; the heat preservation time is 1.5h; then air-cooled to room temperature; the remaining parts of the runner and riser are cut, and the positions of the runner and riser of the casting are polished; The second heating process: the casting is heated to 580℃~585℃, the heating rate is 140~145℃; the holding time is 1.5h; then the casting is cooled to 200℃ in the furnace and taken out of the furnace.

7. The casting process using a sand box as claimed in claim 6, characterized in that: The analysis step also includes a simulation step: simulating the casting and cooling of the casting according to the modeling data to obtain the temperature data in the sand mold cavity during the casting process, T1; Get the temperature data of the sand mold cavity during the cooling process of the casting, T2; The casting steps include: pouring a casting medium into the mold cavity and then cooling it; during the casting process, a heat medium flows into the channel (5); according to the temperature data T1 in the sand mold cavity, the temperature of the heat medium and the interval time of the heat medium flow are adjusted; during the cooling process of the casting, a normal temperature medium flows into the channel (5), and according to the temperature data T2 in the sand mold cavity, the flow rate and the interval time of the normal temperature medium flow are adjusted.

8. The casting process using a sand box as claimed in claim 7, characterized in that: The sand molding step also includes the sand mixing step: The magnesium oxide and the phosphate solution are mixed in a ratio of 2.3:1 to form a mixture, and the mixture is added into the raw sand for stirring, and the mass of the mixture accounts for 8% of the mass of the raw sand.

Citation Information

Patent Citations

  • Improved sand box for special-shaped part and sand mold casting assembly

    CN114453566A

  • Casting forming system and casting process for cooling wall with gas-solid two-phase flow flowing in buried pipe

    CN117961006A

  • Inner wall structure of sand box

    CN202398788U

  • Quick detachable and assemble combination formula sand box

    CN206854604U

  • Rapid cooling sand box

    CN209110134U