Preparation method of metal casting and metal casting

By introducing the function of liquid die forging in the die casting process, dynamically adjusting the filling speed and applying local extrusion, the problems of many pores and easy coating fall off in the die casting process are solved, and the yield and mechanical properties of metal castings are improved, thus achieving The possibility of heat treatment.

CN118926504APending Publication Date: 2024-11-12FOSHAN SHUNDE MIDEA ELECTRICAL HEATING APPLIANCES MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310517736.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The metal castings produced by the existing die-casting process have problems such as many pores, non-density, high waste rate and inability to undergo heat treatment and strengthening, resulting in insufficient product strength and easy coating to fall off.

Method used

Adopt die-casting liquid forging composite process, by preset filling speed and extrusion pressure control in the mold, combined with the liquid mold forging process, dynamically adjust the filling speed and apply local extrusion, reducing the risk of holes and coating foaming, and improving the finished product rate and quality.

Benefits of technology

It significantly reduces the risk of holes and coatings of the product, improves yield and mechanical properties, ensures the internal density and surface quality of metal castings, and supports subsequent heat treatment strengthening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926504A_ABST
    Figure CN118926504A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a metal casting and the metal casting, and the preparation method of the metal casting comprises the steps that a cavity of a mold is filled with molten metal at a preset mold filling speed; and when the molten metal in the cavity of the mold is molded into a semi-molded part, a preset part of the semi-molded part is extruded until the molten metal in the cavity is molded into a metal casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of metal castings, and in particular to a preparation method of a metal casting and the metal casting. Background Art

[0002] Die casting is a metal casting process that uses high pressure to force molten metal into a complex metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate. In addition, the gas involved in the casting during the die casting process will expand when heated, which will cause the die casting to deform and bulge, so that the coating will easily fall off when the casting is subsequently coated. In addition, this type of casting cannot be heat-treated and strengthened later.

[0003] The most commonly used material for cooking utensils is cast aluminum alloy, which is formed through a die-casting process. This type of cooking utensil has the advantages of being light and easy to process, but its hardness and strength are lower than those of steel materials. When used under stress, there is a risk of plastic deformation or local damage. Since products produced by conventional die-casting processes contain pores inside, surface bubbling is very likely to occur after heating, so heat treatment cannot be performed. As a result, the products produced have insufficient strength, and the coating of subsequent molding is not good and is easy to fall off.

[0004] Therefore, how to propose a cooking utensil that can facilitate subsequent coating processing, the processed coating is not easy to fall off, and can be heat-treated and strengthened has become a problem that needs to be solved urgently. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0006] To this end, the first object of the present invention is to provide a method for preparing a metal casting. The second object of the present invention is to provide a metal casting.

[0007] In view of this, the technical solution of the first aspect of the present invention provides a method for preparing a metal casting, comprising: filling molten metal into a mold cavity at a preset filling speed; when the molten metal in the mold cavity is formed into a semi-molded part, extruding a preset portion of the semi-molded part until the molten metal in the cavity is formed into a metal casting.

[0008] According to the preparation method of the metal casting provided by the present invention, when the metal casting is formed, the metal casting is prepared and formed by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly solidified in the mold cavity. After the molten metal is filled, the molten metal will gradually solidify in the mold cavity, and when the molten metal solidifies into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is squeezed until the semi-solid part is formed into a metal casting. In this method, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problem of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing metal castings, the first half of the step adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), so that the two processes of die casting and liquid die forging are combined together, that is, a new process is provided, that is, the die casting liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing the product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking metal castings, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield and quality of the prepared metal castings and reducing their preparation costs.

[0009] Specifically, the semi-molten part, that is, the molten metal, is in a semi-molten state, and the semi-molten state is the state of the material when the temperature is between the solidus and the liquidus of the material.

[0010] In the existing scheme, metal castings are generally formed by die casting. Die casting is a metal casting process. It is a casting method that uses high pressure to force metal melt into a complex metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate. In addition, the gas involved in the casting during the die casting process will expand when heated, which will cause the die casting to deform and bulge, so the die casting cannot be heat-treated and strengthened. However, the metal castings prepared by the present application using the die casting liquid forging composite process have high surface quality, which is specifically reflected in the fact that the surface of the casting is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside. In this way, when the product is subsequently heat-treated, there will be no situation where the gas expands when heated, causing the die casting to deform and bulge, so that the workpiece cast by the present application can be normally heat-treated and strengthened, so that the mechanical properties of the parts can be improved.

[0011] The preparation method also includes: preparing the required molten metal, specifically adding aluminum ingots, quick-dissolving silicon and other raw materials according to the mass percentage of the aluminum alloy components, and then melting the ingredients into an alloy melt. Heating and melting the alloy liquid and degassing and removing slag to obtain the prepared molten metal.

[0012] Furthermore, the method for preparing the metal casting also includes: heat treating the metal casting after the metal casting is demolded. After heat treatment, the strength of the cast parts can be improved. In this way, in the actual process, more suitable materials can be used for processing according to the actual use of the parts. For example, when preparing cooking containers, cast aluminum alloys can be used, and cast aluminum alloys have the advantages of light weight and easy processing, but compared with steel materials, the hardness and strength are lower, and there is a risk of plastic deformation or local damage when used in stress scenarios. Through subsequent heat treatment, the strength of the container formed by the cast aluminum alloy can be improved, making the selection of materials for the container more flexible.

[0013] Furthermore, after the metal casting is demolded, the step of heat treating the metal casting specifically includes: first performing a solution quenching treatment on the metal casting, and then performing an aging treatment on the metal casting.

[0014] Among them, heat treatment specifically includes solution quenching treatment and aging treatment. Experiments have shown that white precipitates are evenly distributed on metal castings after aging treatment. These fine and uniform precipitates provide high strength for metal castings. The performance improvement rate after solution aging heat treatment is more than 30% higher than that of the cast state.

[0015] Furthermore, after the metal casting is heat treated, a precipitation phase is formed on the surface of the metal casting, and the precipitation phase satisfies the following characteristics: the precipitation phase includes a MgZn2 phase and / or a copper-rich phase; and / or the precipitation phase size is greater than or equal to 2 μm and less than or equal to 3 μm.

[0016] In this technical solution, white precipitates are evenly distributed on the metal casting after aging treatment. These precipitates are MgZn2 phases and some copper-rich phases. Specifically, the copper-rich phase is Mg(ZnCu)2 phase. The size of the precipitates is about 2μm-3μm. These small and uniform precipitates form dispersed hard particles, which cause resistance to dislocation movement, thereby providing high strength for the metal casting. It should be noted that the precipitates are related to the material of the molten metal.

[0017] Furthermore, after the metal casting is heat treated, the strength of the metal casting is greater than or equal to 520 MPa and less than or equal to 580 MPa.

[0018] In the above technical solution, in the step of filling the molten metal into the mold cavity at a preset filling speed, the injection pressure is greater than or equal to 65MPa and less than or equal to 110MPa. Further, the injection speed is greater than or equal to 5m / s and less than or equal to 8m / s. Further, the filling time of the molten metal is greater than or equal to 0.02s and less than or equal to 0.05s.

[0019] In this technical solution, when the molten metal is filled into the mold cavity, it is necessary to dynamically adjust the filling speed to control the filling time according to the actual situation, so as to fully control the filling process of the molten metal, and avoid the filling speed being too fast or too slow, which may cause the parts to fail to solidify as required, so as to ensure the quality of the parts after molding, and further reduce the bubbles in the parts, making the parts more dense. By reasonably controlling the specific pressure, injection speed and filling time, high-speed filling of the molten metal can be achieved, so that the molten metal can be cooled quickly. At the same time, by dynamically adjusting the filling speed, air entrainment can be reduced, and the holes in the product after the product is molded can be reduced.

[0020] In the above technical solution, when the preset part of the semi-molded part is extruded, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s. This solution can eliminate shrinkage cavities formed by solidification shrinkage by applying the extrusion force of the above parameters, and obtain high-strength parts with fine and uniform grains and dense structure, thereby ensuring the quality of the parts after molding, and solving the problem of many pores and high scrap rate of die castings.

[0021] Further, the step of filling the molten metal into the mold cavity at a preset filling speed specifically includes: injecting the molten metal at a preset temperature into the mold cavity at a preset filling speed. The preset temperature is greater than the liquidus temperature of the molten metal plus the sum of 50°C-100°C. That is, the preset temperature is greater than or equal to the liquidus temperature of the molten metal plus a temperature threshold, and the temperature threshold is greater than or equal to 50°C and less than or equal to 100°C.

[0022] In the above technical solution, the diameter of the holes in the metal casting is less than or equal to 1.5 mm, and the porosity of the preset holes in the metal casting is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the metal casting is formed, the number of holes in the unit area of ​​10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the metal casting is greater than or equal to twice the diameter of each preset hole itself. This kind of metal casting has relatively few bubbles and the interior of the part is denser, ensuring the qualified rate of the product.

[0023] In the above technical solution, the metal casting includes a container. That is, the metal casting of the present application can be used to prepare containers required for cooking, etc. Of course, it can also be used to prepare other parts.

[0024] In the above technical solution, the molten metal includes a cast aluminum alloy molten metal. In this case, the metal casting includes a cast aluminum alloy part. In particular, when preparing a container required for cooking, the cast aluminum alloy can be used to prepare the container to form a cast aluminum alloy container.

[0025] Furthermore, the molten metal includes an aluminum-silicon alloy melt and / or an aluminum-copper alloy melt and / or an aluminum-zinc-magnesium alloy melt. Therefore, aluminum-silicon alloy castings and / or aluminum-copper alloy castings and / or aluminum-zinc-magnesium alloy castings can be prepared. When preparing metal castings, aluminum-silicon alloy and / or aluminum-copper alloy can be used to prepare different parts, such as preparing containers of different materials, and the parts of these materials can all be processed and formed by the above-mentioned die-casting liquid forging composite process.

[0026] In the above technical solution, the metal casting is a container, and the preparation method further includes: processing the metal casting to a preset size and / or preset accuracy after the metal casting is demolded or after the metal casting is demolded and heat treated; degreasing the metal casting; roughening the inner and outer surfaces of the metal casting until the roughness Ra of the inner and outer surfaces of the metal casting is greater than or equal to 2μm and less than or equal to 5μm; after the roughening treatment, forming a non-stick coating on the inner wall surface of the metal casting.

[0027] In this technical solution, when a metal casting (such as a container) is processed by a die-casting liquid forging composite process, some processing allowances are generally reserved for the metal casting. Therefore, after the metal casting is basically prepared and formed, the metal casting can be processed into the size and accuracy (such as roughness, flatness and coaxiality, etc.) required by the drawing by machining and other methods. Furthermore, the roughness treatment is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. And by performing roughness treatment on the metal casting, the surface quality of the metal casting can be guaranteed, and preparations can be made for subsequent coating spraying on the metal casting. The non-stick performance of the inner wall of the metal casting can be improved by providing a non-stick coating. The non-stick coating can specifically include one or more of PTFE (Polytetrafluoroethylene, Teflon) coating, PFA (Polyfluoroalkoxy, soluble polytetrafluoroethylene) coating, PEEK (Polyetheretherketone, polyetheretherketone) coating, and ceramic coating. Furthermore, after the roughness treatment, a non-stick coating is formed on the inner wall surface of the metal casting, that is, the roughness treatment is performed first and then the non-stick coating is formed. Especially when the metal casting is a container, it is very necessary to spray the non-stick coating on the inner surface. Among them, after the prepared metal casting is processed by machining or roughness treatment, there will be some grease on the surface, so before forming the non-stick coating, it is necessary to perform a degreasing treatment.

[0028] Furthermore, the roughness treatment includes sandblasting. Of course, the roughness treatment may also be other treatment methods such as grinding.

[0029] Furthermore, the degreasing treatment includes heating the metal casting, wherein during the heating treatment, the heating temperature is greater than or equal to 350°C and less than or equal to 420°C, and the heating time is greater than or equal to 8 minutes and less than or equal to 15 minutes. The degreasing treatment can be carried out by high-temperature heating. At this time, the metal casting can be heated, and the specific heating temperature can be 350°C-420°C, and the heating duration can be 8 minutes-15 minutes. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.

[0030] The technical solution of the second aspect of the present invention provides a metal casting, which is prepared by any of the methods provided above. Since the metal casting is prepared by the above preparation method, it has all the beneficial effects of any of the above preparation methods, which will not be repeated here.

[0031] In the above technical solution, the molten metal is prepared from a cast aluminum alloy, and the cast aluminum alloy is prepared by adding aluminum ingots, quick-dissolving silicon and other raw materials according to the mass percentage of the aluminum alloy components.

[0032] The molten metal contains Si, and the weight percentage of Si can be added according to actual needs, and is generally less than or equal to 0.5%.

[0033] In this technical solution, the molten metal for preparing metal castings contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum, but the excessive addition of silicon makes it difficult to obtain a qualified oxide film on the surface of die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide films, and poor oxidation coloring effects. If non-aluminum-silicon alloys are used, the casting performance during die-casting will be extremely poor, not only with a large shrinkage tendency, but also with difficulty in demolding, and it is not suitable for die-casting production at all. Therefore, in the process of preparing metal castings, the present application selects materials containing silicon elements, and controls the weight percentage of silicon within 0.5%, thereby not only ensuring the fluidity of cast aluminum, but also overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production. At the same time, metal castings are manufactured using low-silicon aluminum alloys, so that a uniform and continuous anodized film can be formed on their outer surface, thereby improving the protective effect and surface texture of the prepared products.

[0034] In a specific preparation method, the preparation process is as follows: after the metal casting is formed by the die casting liquid forging composite process, the mold is opened, the metal casting is taken out and cooled. The cooled metal casting is heat treated, specifically including solid solution quenching and aging treatment. Then the heat-treated workpiece is processed to a preset size and / or preset accuracy, and then degreased, and then roughened by sandblasting or other roughness treatment. If the part is a container, it can also be treated with a non-stick coating and then anodized.

[0035] Additional aspects and advantages of the present invention will become apparent from the following description or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 A schematic flow chart of a method for preparing a metal casting according to an embodiment of the present invention is shown;

[0038] Figure 2 Another schematic diagram of the process of preparing a metal casting according to an embodiment of the present invention is shown;

[0039] Figure 3 A schematic diagram showing the structure morphology of a metal casting before heat treatment according to an embodiment of the present invention is shown;

[0040] Figure 4A schematic diagram of the microstructure of a metal casting after heat treatment according to an embodiment of the present invention is shown.

[0041] in, Figure 4 The corresponding relationship between the reference numerals and the component names is as follows:

[0042] 1 Metal casting, 2 Precipitation phase. DETAILED DESCRIPTION

[0043] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0044] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0045] Refer to the following Figures 1 to 4 The preparation method of the metal casting and the metal casting provided by the present invention are described.

[0046] like Figure 1 As shown, an embodiment of the first aspect of the present invention provides a method for preparing a metal casting, comprising:

[0047] S102, filling the molten metal into the mold cavity at a preset filling speed.

[0048] S104, when the molten metal in the cavity of the mold is formed into a semi-formed part, a preset portion of the semi-formed part is extruded until the molten metal in the cavity is formed into a metal casting.

[0049] According to the preparation method of the metal casting provided by the present invention, when the metal casting is formed, the metal casting is prepared and formed by a die-casting liquid forging composite process. Specifically, the preparation steps are: first, the molten metal is filled into the mold cavity of the mold. In this step, the filling speed needs to be fully controlled to ensure that the molten metal can be filled into the mold cavity by high pressure. Specifically, the molten metal is filled into the mold cavity in the way that the molten metal in the die-casting process is filled into the mold cavity, so that the molten metal can be quickly filled into the mold cavity, and the molten metal can be quickly solidified in the mold cavity. After the molten metal is filled, the molten metal will gradually solidify in the mold cavity, and when the molten metal solidifies into a semi-solid part (for example, after the filling is completed for a preset time), the preset part of the semi-solid part is squeezed until the semi-solid part is formed into a metal casting. In this method, after the molten metal solidifies into a semi-solid part, the semi-solid part is locally extruded until the end, and this method is similar to the liquid die forging process, which greatly solves the problem of many pores, non-density and high scrap rate of parts formed by the die casting process. That is, in the process of preparing metal castings, the first half of the step adopts the die casting process, and the liquid die forging process is combined in the latter step (specifically reflected in the local extrusion of the semi-solid part), so that the two processes of die casting and liquid die forging are combined together, that is, a new process is provided, that is, the die casting liquid forging composite process. This process, through targeted transformation of the die casting technology, injects the function of liquid die forging, reduces air entrainment by dynamically adjusting the filling speed (filling time) during the die casting process, and uses the extrusion rod in the mold to locally extrude and compensate the shrinkage of the semi-solid casting when the metal solidifies and shrinks, thereby greatly reducing the product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience. In this way, the respective advantages of low die casting cost and high liquid die forging casting quality are utilized, and the die casting-liquid die forging composite process is creatively used to manufacture cooking metal castings, thereby improving the yield rate of the original die-casting aluminum alloy and improving the cost performance, thereby ensuring the yield and quality of the prepared metal castings and reducing their preparation costs.

[0050] In the existing scheme, metal castings are generally formed by die casting. Die casting is a metal casting process. It is a casting method that uses high pressure to force metal melt into a complex metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate. In addition, the gas involved in the casting during the die casting process will expand when heated, which will cause the die casting to deform and bulge, so the die casting cannot be heat-treated and strengthened. However, the metal castings prepared by the present application using the die casting liquid forging composite process have high surface quality, which is specifically reflected in the fact that the surface of the casting is not easy to bubble, and pores or shrinkage holes are not easy to be generated inside. In this way, when the product is subsequently heat-treated, there will be no situation where the gas expands when heated, causing the die casting to deform and bulge, so that the workpiece cast by the present application can be normally heat-treated and strengthened, so that the mechanical properties of the parts can be improved.

[0051] The preparation method also includes: preparing the required molten metal, specifically adding aluminum ingots, quick-dissolving silicon and other raw materials according to the mass percentage of the aluminum alloy components, and then melting the ingredients into an alloy melt. Heating and melting the alloy liquid and degassing and removing slag to obtain the prepared molten metal.

[0052] Furthermore, if Figure 2 As shown, the method for preparing the metal casting also includes: S106, heat treating the metal casting after the metal casting is ejected from the mold.

[0053] After heat treatment, the strength of cast parts can be improved. In this way, in the actual process, more suitable materials can be used for processing according to the actual use of the parts. For example, when preparing cooking containers, cast aluminum alloys can be used. Cast aluminum alloys have the advantages of light weight and easy processing, but compared with steel materials, they have lower hardness and strength. There is a risk of plastic deformation or local damage when used in stress scenarios. Subsequent heat treatment can improve the strength of containers made of cast aluminum alloys, making the selection of containers more flexible.

[0054] Furthermore, after the metal casting is demolded, the step of heat treating the metal casting specifically includes: first performing a solution quenching treatment on the metal casting, and then performing an aging treatment on the metal casting.

[0055] The heat treatment specifically includes solution quenching treatment and aging treatment. Experiments have shown that white precipitates 2 are evenly distributed on the metal casting 1 after aging treatment. These fine and uniform precipitates 2 provide high strength for the metal casting 1. The performance improvement rate after solution aging heat treatment is more than 30% higher than that of the cast state.

[0056] Among them, the microstructure of metal castings after heat treatment is as follows Figure 4 As shown in the figure, the microstructure before heat treatment is as follows Figure 3 By comparison Figure 3 and Figure 4 It can be seen that after the metal casting 1 is heat treated, a white precipitate phase 2 is formed on the surface of the metal casting 1. Further, the precipitate phase 2 meets the following characteristics: the precipitate phase 2 includes a MgZn2 phase and a copper-rich phase; and / or the size of the precipitate phase 2 is greater than or equal to 2 μm and less than or equal to 3 μm.

[0057] In this embodiment, the white precipitated phase 2 (such as Figure 4 As shown), these precipitated phases 2 are MgZn2 phases and some copper-rich phases Mg(ZnCu)2 phases. The size of the precipitated phases 2 is about 2μm-3μm. These fine and uniform precipitated phases 2 form dispersed hard particles, which create resistance to dislocation movement, thereby providing high strength to the metal casting 1.

[0058] Furthermore, after the metal casting is heat treated, the strength of the metal casting is greater than or equal to 520 MPa and less than or equal to 580 MPa.

[0059] In the above embodiment, in the step of filling the molten metal into the mold cavity at a preset filling speed, the specific pressure is greater than or equal to 65 MPa and less than or equal to 110 MPa. Further, the injection speed is greater than or equal to 5 m / s and less than or equal to 8 m / s. Further, the filling time of the molten metal is greater than or equal to 0.02 s and less than or equal to 0.05 s.

[0060] In this embodiment, when the molten metal is specifically filled into the mold cavity, it is necessary to dynamically adjust the filling speed to control the filling time in combination with the actual situation, so as to fully control the filling process of the molten metal, and avoid the filling speed being too fast or too slow, which may cause the parts to fail to solidify as required, so as to ensure the quality of the parts after molding, and further reduce the bubbles in the parts, making the parts more dense. By reasonably controlling the specific pressure, injection speed and filling time, high-speed filling of the molten metal can be achieved, so that the molten metal can be quickly cooled. At the same time, by dynamically adjusting the filling speed, air entrainment can also be reduced, and the holes in the product after the product is molded can be reduced.

[0061] In the above embodiment, when the preset part of the semi-molded part is extruded, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s. In this scheme, by applying the extrusion force of the above parameters, the shrinkage cavity formed by solidification shrinkage can be eliminated, and a high-strength component with fine and uniform grains and dense structure can be obtained, thereby ensuring the quality of the formed parts and solving the problem of many pores and high scrap rate of die-cast parts.

[0062] Specifically, the filling speed of the molten metal is controlled below 0.8 m / s.

[0063] Further, the step of filling the molten metal into the mold cavity at a preset filling speed specifically includes: injecting the molten metal at a preset temperature into the mold cavity at a preset filling speed. The preset temperature is greater than the liquidus temperature of the molten metal plus the sum of 50°C-100°C. That is, the preset temperature is greater than or equal to the liquidus temperature of the molten metal plus a temperature threshold, and the temperature threshold is greater than or equal to 50°C and less than or equal to 100°C.

[0064] In the above embodiment, the diameter of the hole in the metal casting is less than or equal to 1.5 mm, and the porosity of the preset holes in the metal casting is greater than 0 and less than or equal to 0.5%. Specifically, when calculating the holes, holes with a diameter less than 0.25 mm are not counted. After the metal casting is formed, the number of holes in a unit area of ​​10 cm × 10 cm is no more than 4, and the distance between two holes is not less than 5 cm. The diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each preset hole and the outer surface of the metal casting is greater than or equal to twice the diameter of each preset hole itself. This kind of metal casting has fewer bubbles and the interior of the part is denser, ensuring the qualified rate of the product.

[0065] In the above embodiment, the metal casting includes a container. That is, the metal casting of the present application can be used to prepare containers required for cooking, etc. Of course, it can also be used to prepare other parts.

[0066] In the above embodiment, the molten metal includes a cast aluminum alloy molten metal. In this case, the metal casting includes a cast aluminum alloy part. In particular, when preparing a container required for cooking, the cast aluminum alloy can be used to prepare the container to form a cast aluminum alloy container.

[0067] Furthermore, the molten metal includes an aluminum-silicon alloy melt and / or an aluminum-copper alloy melt. Therefore, aluminum-silicon alloy castings and / or aluminum-copper alloy castings can be prepared. When preparing metal castings, aluminum-silicon alloy and / or aluminum-copper alloy can be used to prepare different parts, such as preparing containers of different materials, and the parts of these materials can all be processed and formed by the above-mentioned die-casting liquid forging composite process.

[0068] In the above embodiment, the metal casting is a container, and the preparation method further includes: processing the metal casting to a preset size and / or preset accuracy after the metal casting is demolded or after the metal casting is demolded and heat treated; degreasing the metal casting; performing roughness treatment on the inner and outer surfaces of the metal casting until the roughness Ra of the inner and outer surfaces of the metal casting is greater than or equal to 2μm and less than or equal to 5μm; after the roughness treatment, forming a non-stick coating on the inner wall surface of the metal casting.

[0069] In this embodiment, when a metal casting (such as a container) is processed by a die-casting liquid forging composite process, some processing allowances are generally reserved for the metal casting. Therefore, after the metal casting is basically prepared and formed, the metal casting can be processed into the size and accuracy (such as roughness, flatness and coaxiality, etc.) required by the drawing by machining and other methods. Further, the roughness treatment is generally performed after the demolding pretreatment. If there is no demolding pretreatment step, the roughness treatment can be performed directly after the part is demolded. And by performing roughness treatment on the metal casting, the surface quality of the metal casting can be guaranteed, and preparations can be made for subsequent coating spraying on the metal casting. The non-stick performance of the inner wall surface of the metal casting can be improved by setting a non-stick coating. The non-stick coating can specifically include one or more of PTFE coating, PFA coating, PEEK coating, and ceramic coating. Further, after the roughness treatment, a non-stick coating is formed on the inner wall surface of the metal casting, that is, the roughness treatment is performed first, and then the non-stick coating is formed. In particular, when the metal casting is a container, it is very necessary to spray a non-stick coating on the inner surface. Among them, after the prepared metal castings are processed by machining or roughening, there will be some grease on the surface, so degreasing treatment is required before forming the non-stick coating.

[0070] Furthermore, the roughness treatment includes sandblasting. Of course, the roughness treatment may also be other treatment methods such as grinding.

[0071] Furthermore, the degreasing treatment includes heating the metal casting, wherein during the heating treatment, the heating temperature is greater than or equal to 350°C and less than or equal to 420°C, and the heating time is greater than or equal to 8 minutes and less than or equal to 15 minutes. The degreasing treatment can be carried out by high-temperature heating. At this time, the metal casting can be heated, and the specific heating temperature can be 350°C-420°C, and the heating duration can be 8 minutes-15 minutes. Of course, the degreasing treatment can also be carried out by other methods such as chemical degreasing.

[0072] like Figure 4 As shown, an embodiment of the second aspect of the present invention provides a metal casting, which is prepared by any of the methods provided above. Since the metal casting is prepared by the above preparation method, it has all the beneficial effects of any of the above preparation methods, which will not be repeated here. Furthermore, a white precipitate phase 2 is formed on the prepared metal casting 1.

[0073] In the above embodiment, the molten metal is prepared from a cast aluminum alloy, and the cast aluminum alloy is prepared by adding raw materials such as aluminum ingots and quick-dissolving silicon according to the mass percentage of the aluminum alloy components.

[0074] The molten metal contains Si, and the weight percentage of Si can be added according to actual needs, and is generally less than or equal to 0.5%.

[0075] In this embodiment, the molten metal for preparing the metal casting contains silicon, and the weight percentage of silicon is less than 0.5%. Because, in order to pursue good formability, die-casting products often use die-cast aluminum with a high silicon content, and the presence of silicon can improve the fluidity of cast aluminum, but the excessive addition of silicon makes it difficult to obtain a qualified oxide film on the surface of die-cast aluminum, which is specifically manifested as discontinuous and non-dense oxide films, and poor oxidation coloring effect. If non-aluminum-silicon alloys are used, the casting performance during die-casting will be extremely poor, not only with a large shrinkage tendency, but also difficult to demold, and not suitable for die-casting production at all. Therefore, in the process of preparing metal castings, the present application selects materials containing silicon elements, and controls the weight percentage of silicon within 0.5%, thereby not only ensuring the fluidity of cast aluminum, but also overcoming the shortcoming that non-aluminum-silicon alloys have poor fluidity and are not suitable for die-casting production. At the same time, metal castings are manufactured using low-silicon aluminum alloys, so that a uniform and continuous anodized film can be formed on their outer surface, thereby improving the protection effect and surface texture of the prepared products.

[0076] In a specific preparation method, the preparation process is as follows: after the metal casting is formed by the die casting liquid forging composite process, the mold is opened, the metal casting is taken out and cooled. The cooled metal casting is heat treated, specifically including solution quenching and aging treatment. Then the heat-treated workpiece is processed to a preset size and / or preset accuracy. Then degreasing treatment is performed, and then roughness treatment such as sandblasting is performed. If the part is a container, a non-stick coating treatment can be performed at the end, and then anodizing treatment is performed.

[0077] The following uses die-cast aluminum as an example to further introduce the method for preparing a metal casting provided by the present application and the metal casting prepared by the method. Specifically:

[0078] Among them, the die casting-liquid forging composite process includes the following steps:

[0079] Step 1: Add aluminum ingots, quick-dissolving silicon and other raw materials according to the mass percentage of aluminum alloy components for batching;

[0080] Step 2: After heating and melting the alloy liquid and removing gas and slag, the molten metal is injected into the mold cavity at 50℃-100℃ above the liquidus temperature of the selected aluminum alloy, and then the die casting-liquid forging composite process is used to form the corresponding workpiece;

[0081] The third step: heat treatment of the aluminum alloy after composite forming, specifically solid solution + aging;

[0082] Step 4: Finish the inner and outer surfaces of the cooking vessel, and then perform high-temperature degreasing and non-stick coating treatment. The heating temperature for high-temperature degreasing is 350℃-420℃, and the heating time is 8min-15min;

[0083] Among them, the die-casting-liquid forging composite process hydraulically injects molten aluminum into the mold cavity, dynamically adjusts the filling speed to reduce air entrapment, and then uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting formed in the cavity to increase its density.

[0084] Specifically, the cast aluminum alloy is selected from aluminum-silicon alloy, aluminum-copper alloy, etc., which can be formed into a high-density aluminum alloy through a die-casting-liquid forging composite process and can be strengthened by heat treatment.

[0085] The maximum diameter of a single hole inside a cooking vessel produced by the die-casting-liquid forging composite process shall not exceed 1.5mm, and holes with a diameter less than 0.25mm shall not be counted. In a unit area of ​​10cm×10cm, the number of holes shall not exceed 4, and the distance between two holes shall not be less than 5cm, and the distance between the center point of the hole and the surface of the casting shall not be less than 2 times the diameter of the hole itself.

[0086] Specifically, according to the above pore characteristics, the cast aluminum alloy is first subjected to solution quenching treatment and then to aging treatment. During the aging treatment, the supersaturated solid solution formed during the solution treatment tends to spontaneously decompose and segregate, first forming the GP zone, then the metastable phase, and finally the equilibrium phase, that is, the final precipitation phase.

[0087] The die casting-liquid forging composite process can be used to heat treat and strengthen the aluminum-zinc-magnesium alloy. The microstructure morphology of the aluminum-zinc-magnesium alloy after solution quenching is as follows: Figure 3 As shown in the figure, there is no visible second phase in the alloy matrix, indicating that the effect of the solution treatment is very good. The white precipitate phase 2( Figure 4 ), these fine and uniform precipitates provide high strength to the aluminum alloy.

[0088] Aluminum-zinc-magnesium alloys include 7075. After 7075 is formed by a die-casting-liquid forging composite process and heat treated, its ultimate tensile strength can reach 520MPa-580MPa. Its mechanical properties are equivalent to those of 304 stainless steel. At the same time, it is light in weight, easy to process and not prone to plastic deformation.

[0089] Specifically, when the die-cast aluminum is a cooking utensil, its preparation method includes: processing the cooking utensil through a die-casting liquid forging composite process, processing the cooking utensil to a specified size and precision according to the drawing requirements after it is removed from the mold and cooled, and then operating according to the following process flow: (1) sandblasting the inside and outside of the cooking utensil, and the surface roughness Ra after sandblasting is: 2μm-5μm; (2) high-temperature heating for high-temperature degreasing, the heating temperature is 350℃-420℃, and the heating time is 8min-15min; (3) spraying a non-stick coating on the inside of the cooking utensil, including but not limited to PTFE, PFA, PEEK, ceramics and other coatings that can achieve non-stick properties.

[0090] This technology combines the two processes of die casting and liquid die forging, taking advantage of the respective advantages of low die casting cost and high liquid die forging casting quality, and creatively uses the die casting-liquid die forging composite process to manufacture cooking utensils, thereby improving the yield of the original die-casting aluminum alloy and enhancing the cost-effectiveness.

[0091] Die casting is a metal casting process that uses high pressure to force molten metal into a complex-shaped metal mold. It has the characteristics of high-speed filling and rapid cooling, but it has many pores, is not dense, and has a high scrap rate.

[0092] Liquid die forging is a metal forming process that has both casting characteristics and is similar to die forging. It is a process in which a certain amount of molten metal is directly poured into the mold cavity and solidified under the action of continuous mechanical static pressure. Liquid die forging technology can eliminate shrinkage cavities formed by solidification shrinkage and obtain high-strength parts with fine and uniform grains and dense structure, but the cost is relatively high.

[0093] The die-casting-liquid forging composite process injects the function of liquid forging by making targeted modifications to the die-casting technology. It reduces air entrapment by dynamically adjusting the filling speed during the die-casting process, and uses the extrusion rod in the mold to locally extrude and compensate for the shrinkage of the semi-solid casting when the metal solidifies and shrinks. This greatly reduces product holes, and the risk of blistering or local shedding of the coating is significantly reduced, which not only improves the product qualification rate, but also enhances the user experience.

[0094] Specifically, the present application tests Examples 1 to 3 and Comparative Example 1:

[0095] Example 1: Aluminum-silicon alloy cooking utensils were manufactured by die casting-liquid forging composite process, and the content of each element was as follows: Si: 8.8, Mg: 0.25, Mn: 0.35, Al: balance. The heat treatment process after composite process molding was as follows: put it into the heating furnace and evenly heat it to 535℃ at a rate of 10℃ / min, keep it warm for 2h, then take it out and water cool it; after cooling to room temperature, continue to put it into the furnace and heat it to 175℃ at a rate of 5℃ / min, keep it warm for 8h, then take it out and air cool it to room temperature.

[0096] Example 2: Aluminum-copper alloy cooking utensils were manufactured by die casting-liquid forging composite process, and the content of each element was as follows: Cu: 5.0, Mn: 0.7, Ti: 0.25, Al: balance. The heat treatment process after composite process molding was as follows: put it into the heating furnace and evenly heat it to 535℃ at a rate of 10℃ / min, keep it warm for 5h, then take it out and water cool it; after cooling to room temperature, continue to put it into the furnace and heat it to 175℃ at a rate of 5℃ / min, keep it warm for 3h, then take it out and air cool it to room temperature.

[0097] Example 3: Aluminum-magnesium-zinc alloy cooking utensils were manufactured by die casting-liquid forging composite process, and the content of each element was as follows: Zn: 5.9, Mg: 2.4, Cu: 1.5, Cr: 0.19, Al: balance. The heat treatment process after composite process molding was as follows: put it into the heating furnace and evenly heat it to 470℃ at a rate of 10℃ / min, keep it warm for 2h, then take it out and water cool it; after cooling to room temperature, continue to put it into the furnace and heat it to 120℃ at a rate of 5℃ / min, keep it warm for 16h, then take it out and air cool it to room temperature.

[0098] Comparative Example 1: After Japanese brand ADC12 die-cast aluminum was formed using the traditional die-casting process, it was heated according to the heat treatment process of Example 1. It was found that the surface of the vessel was obviously bubbled and could not be used normally, so it was scrapped.

[0099] Test method: 5 cooking utensils of each embodiment are taken before and after heat treatment. All samples are sampled at the same location with a sample size of 10 mm×50 mm×3 mm. Then tensile strength, yield strength, elongation and Vickers hardness tests are carried out, and the data results are averaged.

[0100] Table 1: Comparison of mechanical properties of samples before and after heat treatment

[0101]

[0102] It can be seen from the examples and comparative examples in Table 1 that the aluminum alloy castings produced by the die casting-liquid forging composite process can be heat treated without problems, and the strength and hardness after heat treatment will be significantly improved. After heat treatment, the products produced by the traditional die casting process will have obvious bubbling after heating due to the presence of many pores and defects inside the castings during the die casting process, and the products cannot be used.

[0103] In the description of this specification, the terms "connection", "installation", "fixation" and the like should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0104] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0105] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a metal casting, characterized in that: include: Filling the molten metal into the mold cavity at a preset filling speed; When the molten metal in the cavity of the mold is formed into a semi-molded part, a preset portion of the semi-molded part is extruded until the molten metal in the cavity is formed into the metal casting.

2. The method for preparing a metal casting according to claim 1, characterized in that: Also includes: After the metal casting is demolded, the metal casting is heat treated.

3. The method for preparing a metal casting according to claim 2, characterized in that: The step of heat treating the metal casting after the metal casting is ejected from the mold specifically includes: The metal casting is first subjected to a solution quenching treatment and then to an aging treatment.

4. The method for preparing a metal casting according to claim 2, characterized in that: After the metal casting is heat treated, a precipitated phase is formed on the surface of the metal casting, and the precipitated phase meets the following characteristics: The precipitated phase includes a MgZn2 phase and / or a copper-rich phase; and / or The size of the precipitated phase is greater than or equal to 2 μm and less than or equal to 3 μm, Wherein, after the metal casting is heat treated, the strength of the metal casting is greater than or equal to 520 MPa and less than or equal to 580 MPa.

5. The method for preparing a metal casting according to claim 1, characterized in that: In the step of filling the molten metal into the mold cavity at a preset filling speed, the injection pressure is greater than or equal to 65 MPa and less than or equal to 110 MPa, the injection speed is greater than or equal to 5 m / s and less than or equal to 8 m / s, and the filling time of the molten metal is greater than or equal to 0.02 and less than or equal to 0.05 s; and / or When extruding the preset part of the semi-formed part, the extrusion pressure is greater than or equal to 60MPa and less than or equal to 100MPa, the pressurization speed is greater than or equal to 0.1m / s and less than or equal to 0.4m / s, and the extrusion time is greater than or equal to 10s and less than or equal to 30s.

6. The method for preparing a metal casting according to claim 1, characterized in that: The step of filling the molten metal into the mold cavity at a preset filling speed specifically includes: A molten metal at a preset temperature is injected into the cavity at a preset filling speed, wherein the preset temperature is greater than or equal to the liquidus temperature of the molten metal plus a temperature threshold, and the temperature threshold is greater than or equal to 50°C and less than or equal to 100°C.

7. The method for preparing a metal casting according to claim 1, characterized in that: The diameter of the hole in the metal casting is less than or equal to 1.5 mm, the porosity of the preset holes in the metal casting is greater than 0 and less than or equal to 0.5%, the diameter of the preset holes is greater than 0.25 mm and less than or equal to 1.5 mm, and the distance between each of the preset holes and the outer surface of the metal casting is greater than or equal to twice the diameter of each of the preset holes.

8. The method for preparing a metal casting according to any one of claims 1 to 7, characterized in that: The metal casting comprises a container; and / or The molten metal includes a cast aluminum alloy molten metal.

9. The method for preparing a metal casting according to any one of claims 1 to 7, characterized in that: The molten metal includes an aluminum-silicon alloy melt and / or an aluminum-copper alloy melt and / or an aluminum-zinc-magnesium alloy melt.

10. The method for preparing a metal casting according to any one of claims 1 to 7, characterized in that: The metal casting is a container, and the preparation method further comprises: After the metal casting is demolded or after the metal casting is demolded and heat treated, processing the metal casting to a preset size and / or a preset accuracy; Degreasing the metal casting; Performing roughness treatment on the inner and outer surfaces of the metal casting until the roughness Ra of the inner and outer surfaces of the metal casting is greater than or equal to 2 μm and less than or equal to 5 μm; After the roughening treatment, a non-stick coating is formed on the inner wall surface of the metal casting.

11. The method for preparing a metal casting according to claim 10, characterized in that: The roughness treatment comprises sandblasting; and / or The degreasing treatment includes heating the metal casting, wherein during the heating treatment, the heating temperature is greater than or equal to 350° C. and less than or equal to 420° C., and the heating time is greater than or equal to 8 minutes and less than or equal to 15 minutes.

12. A metal casting, characterized in that: The metal casting is prepared by the method for preparing a metal casting according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Non-stick coating, preparation method, cookware and cooking equipment

    CN109252126A

  • Seven-series aluminum alloy small piece and die casting method thereof

    CN109877289A

  • Seven-series aluminum alloy small part and die-casting die thereof

    CN109877291A

  • High-strength aluminum alloy and extrusion casting preparation method