Additive manufacturing method for ultrasonic vibration assisted laser melting deposition
By synchronously using ultrasonic vibration during laser melting and deposition, the problem of sample differences and unfusion defects between different equipment is solved, more efficient material manufacturing and wider process windows are achieved, and mechanical properties and equipment versatility are improved.
Patent Information
- Application Number
- CN202410994821.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing laser melting and deposition technology, the samples printed with the same parameters vary greatly between different equipment, especially when the laser power is insufficient, the unfusion defect is serious, which limits the process window and the utilization efficiency of the material.
Ultrasonic vibration is used simultaneously during the laser melting and deposition process, and the ultrasonic impact head is used to move synchronously with the laser through the ultrasonic impact head, adjust the amplitude and offset distance, assist in melting and deposition, reduce unfusion defects and expand the process window.
Significantly suppress unfusion defects, improve the mechanical properties of the material, expand the process window, reduce post-processing time, improve the universality of the equipment and the optimization efficiency of process parameters.
Smart Images

Figure CN118926545A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to an additive manufacturing method utilizing ultrasonic vibration to assist laser melting deposition. Background Art
[0002] Laser melting deposition (LMD) is a process that uses lasers to melt metal raw materials to create new parts or modify the geometry of existing parts. Compared with traditional manufacturing technologies, laser melting deposition shortens product development time, can manufacture parts with complex structures, improves raw material utilization efficiency and reduces energy consumption, and is widely used in titanium alloy manufacturing.
[0003] At the same time, due to the limited number of manufacturers of commercial laser melting deposition machines, many users design and integrate the components required for laser melting deposition by themselves, and there are great differences between different integrated devices. For example, the type and wavelength of the laser vary between different laser melting deposition machines, including fiber, CO2 or Nd:YAG lasers, with powers ranging from 1 to 5kW. The main problem arising from this is that the optimal printing parameters studied by different devices vary a lot, and the samples printed by different devices with the same parameters vary greatly. Especially when the laser power is limited, the lack of fusion defect is an unavoidable problem. For alloys with higher melting points or difficult to weld, the range of the process window is therefore limited.
[0004] At present, existing technologies mainly improve defects by introducing post-processing to optimize its performance. For example, the titanium alloy manufactured by additive manufacturing is heated to a predetermined temperature, and then pressure is applied at both ends to close the defects generated during the printing process. However, this post-processing will increase processing time and energy consumption, significantly reducing the efficiency of additive manufacturing.
[0005] Therefore, it is of great significance to develop laser melting deposition processing methods that do not require additional post-processing to improve defects in additively manufactured alloys and expand the process window. Summary of the invention
[0006] The purpose of the present invention is to provide an ultrasonic vibration assisted laser melting deposition additive manufacturing method to solve the problem of unfused defects in existing laser melting deposition samples.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] The present invention provides an ultrasonic vibration assisted laser melting deposition additive manufacturing method, comprising the following steps:
[0009] During the laser melting deposition process, ultrasonic vibration is simultaneously used to ultrasonically treat the laser melting deposition area for additive manufacturing.
[0010] Furthermore, the laser power of the laser melting deposition is 1000-2400W; the amplitude of the ultrasonic vibration is 0-100%, and is not 0%.
[0011] Furthermore, the material used for the additive manufacturing is titanium alloy, titanium-based composite material, stainless steel or NiTi alloy.
[0012] Furthermore, the titanium alloy is Ti6Al4V alloy.
[0013] Furthermore, powder or wire is used for the additive manufacturing.
[0014] Furthermore, when powder is used for the additive manufacturing, the powder feeding gas in the laser melting deposition process is argon.
[0015] Furthermore, synchronously using ultrasonic vibration in the laser melting deposition process specifically includes: moving the ultrasonic impact head and the laser of the laser melting deposition equipment at the same movement speed to perform ultrasonic vibration-assisted laser melting deposition.
[0016] Furthermore, the offset distance between the ultrasonic impact head and the laser is 30-80 mm.
[0017] Furthermore, the scanning speed during the deposition process is 100-500 mm / min, and the powder feeding rate is 11.2 g / min-19.6 g / min.
[0018] In the present invention, 20 kHz ultrasonic vibration is more preferably used.
[0019] The front end portion (the length of which is the offset distance between the ultrasonic impact head and the laser) of the product produced by the present invention has not been ultrasonically treated, and this portion can be selectively cut off.
[0020] The more preferred manufacturing method of the present invention is as follows:
[0021] (1) Grind the substrate clean with an angle grinder, clean the stains on the surface, fix it on the workbench, seal the argon filling chamber, and fill it with high-purity argon gas.
[0022] (2) The Ti6Al4V alloy powder used is produced by a plasma rotating electrode method, and the model specification is -60+200 mesh. The Ti6Al4V alloy powder is poured into a powder feeder, and the powder feeding gas is high-purity argon.
[0023] (3) Fix the ultrasonic impact head and the laser together so that they can move at the same speed. Adjust the offset distance between the ultrasonic impact head and the laser and the amplitude of the ultrasonic vibration. The offset distance ranges from 30 to 80 mm. The amplitude of the ultrasonic assistance is expressed as a percentage, ranging from 0 to 100%.
[0024] (4) Depending on the material, the laser power selection range is 1000-2400W, the scanning speed is 100-500mm / min, the powder feeding rate is 11.2g / min-19.6g / min, and the laser lifting height is defined according to different process parameters, ranging from 0.8-1.4mm.
[0025] (5) In order to ensure that the interlayer residence time of each point in each layer is the same, a unidirectional deposition strategy is adopted. The laser moves along a predetermined direction to melt the powder sprayed from the nozzle. After the laser moves a certain distance, the ultrasonic impact head falls at the starting point to act on the solidified single wall and moves at the same speed as the laser. When the laser moves to the end, the two systems stop working at the same time.
[0026] (6) The ultrasonic impact head and the laser move synchronously back to the starting point and repeat the above steps until the predetermined number of layers is reached.
[0027] (7) Take out the substrate and sample after they have cooled to room temperature.
[0028] The present invention also provides a material prepared by the additive manufacturing method.
[0029] The present invention is based on laser melting deposition and is supplemented with synchronous ultrasonic vibration. Ultrasonic waves are transmitted through solids into the liquid molten pool, which can produce cavitation and acoustic streaming effects. In the present invention, the ultrasonic impact head and the laser move synchronously, which can ensure that the ultrasonic vibration effect on the molten pool is not attenuated by the length and height of the sample, and also saves the time of post-processing.
[0030] Usually, in the additive manufacturing process, when the laser power is too low, the molten pool is shallow and narrow, and the powder that is not fully melted remains in the molten pool, so that each two layers cannot be fully metallurgically bonded, resulting in unfused defects between each two layers. The length of the unfused defects can reach tens of microns to several millimeters, and the shape is irregular. Unmelted powder may be contained inside the unfused. When ultrasonic vibration acts in the molten pool, due to the cavitation effect and vibration, the molten pool is strongly stirred, driving the unmelted powder in the molten pool to flow, increasing the powder's absorption of the laser heat source and reducing the chance of defect formation. And by stirring the molten pool, the heat exchange between layers is increased, so that the previously solidified deposited layer is heated again, and each two layers are metallurgically bonded again, resulting in a denser sample. In addition, due to the effect of acoustic streaming, the flow of the molten pool is enhanced, which will cause the liquid alloy to move to the lower layer and fill the unfused defects. Although ultrasonic vibration suppresses unfused defects, there are still a small number of powder particles that are not completely melted, and the ultrasonic cavitation effect leads to the formation of cavitation bubbles, and a small amount of protective gas enters the molten pool to form pores due to the strong stirring effect. Due to the stirring effect of ultrasonic vibration on the molten pool, the cooling rate increases, and some gases do not have time to escape, resulting in microscopic spherical gas pores. In contrast, the volume of unfused defects is larger, presenting an irregular wedge or ribbon shape, with sharp ends. According to the research of Truong et al., the sharp grooves formed in the unfused defects will promote the initiation and expansion of cracks, and stress concentration is easily formed during uniaxial tension, resulting in faster failure, while the pores are round and the number is small, which can alleviate stress concentration and have less impact on mechanical properties. Therefore, eliminating unfused defects can improve mechanical properties. Compared with traditional additive manufacturing and its post-processing, the present invention uses synchronous ultrasonic vibration to significantly suppress unfused defects and expand the process window. The equipment can be installed in different laser melting deposition systems, saving the cost of optimizing process parameters and increasing the versatility of process parameters between different equipment.
[0031] The present invention discloses the following technical effects:
[0032] The present invention utilizes ultrasonic vibration to assist laser melting deposition for material additive manufacturing. The use of synchronous ultrasonic vibration can significantly suppress the unfused defects of alloy materials and expand the process window. The equipment can be installed in different laser melting deposition systems, saving the cost of optimizing process parameters and increasing the versatility of process parameters between different equipment.
[0033] In the additive manufacturing process of the present invention, the ultrasonic impact head and the laser move synchronously. Compared with traditional post-processing, no additional post-processing time is required, and it can be ensured that the effect of ultrasound does not decay with the increase of sample height and length.
[0034] The device of the present invention is simple and has strong versatility, can be used on different devices, suppresses defects, and expands the process window of additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 The microstructure diagrams of Ti6Al4V alloys prepared in Comparative Example 1(a) and Example 1(b) of the present invention;
[0037] Figure 2 1 and 1 are stress-strain curves of Ti6Al4V alloys prepared in Comparative Example 1 and Example 1 of the present invention in different directions. DETAILED DESCRIPTION
[0038] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0039] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0040] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0041] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0042] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0043] The present invention is further described in detail below in conjunction with the accompanying drawings and specific implementations. The technical solution of the present invention is not limited to the specific implementations listed below.
[0044] Example 1
[0045] (1) The Ti6Al4V alloy substrate is polished clean with an angle grinder to remove stains on the surface, fixed on a workbench, and the argon filling chamber is sealed and filled with high-purity argon gas.
[0046] (2) Pour Ti6Al4V alloy powder (model specification is -60+200 mesh, produced by plasma rotating electrode method) into the powder feeder, and the powder feeding gas is high-purity argon.
[0047] (3) Fix the ultrasonic impact head and the laser together so that they can move at the same speed. Adjust the offset distance between the ultrasonic impact head and the laser and the amplitude of the ultrasonic vibration so that the offset distance is 40 mm, the amplitude of the ultrasonic vibration is 100%, and the frequency of the ultrasonic vibration is 20 kHz.
[0048] (4) The laser power was selected as 1240 W, the scanning speed was 300 mm / min, the powder feeding rate was 16.8 g / min, the lifting height of the laser was 1.0 mm, and the length of the sample was set to 150 mm.
[0049] (5) In order to ensure that the interlayer residence time of each point in each layer is the same, a unidirectional deposition strategy is adopted. The laser moves along a predetermined direction to melt the powder sprayed from the nozzle. After the laser moves a certain distance, the ultrasonic impact head falls at the starting point and moves at the same speed as the laser. When the laser moves to the end, the two systems stop working at the same time.
[0050] (6) The laser returns to the starting point and repeats the above steps until the predetermined number of layers is reached.
[0051] (7) Take out the substrate and sample after they have cooled to room temperature.
[0052] Comparative Example 1
[0053] The only difference from Example 1 is that no ultrasonic treatment is performed. The specific steps are as follows:
[0054] (1) The Ti6Al4V alloy substrate is polished clean with an angle grinder to remove stains on the surface, fixed on a workbench, and the argon filling chamber is sealed and filled with high-purity argon gas.
[0055] (2) Pour Ti6Al4V alloy powder (model specification is -60+200 mesh, produced by plasma rotating electrode method) into the powder feeder, and the powder feeding gas is high-purity argon.
[0056] (3) The laser power was selected as 1240 W, the scanning speed was 300 mm / min, the powder feeding rate was 16.8 g / min, the lifting height of the laser was 1.0 mm, and the length of the sample was set to 150 mm.
[0057] (4) In order to ensure that the interlayer residence time of each point in each layer is the same, a unidirectional deposition strategy is adopted, and the laser moves along the predetermined direction to melt the powder ejected from the nozzle.
[0058] (5) The laser returns to the starting point and repeats the above steps until the predetermined number of layers is reached.
[0059] (6) Take out the substrate and sample after they have cooled to room temperature.
[0060] Figure 1 The microstructure diagrams of Ti6Al4V alloys prepared in the deposited state (Comparative Example 1) and by ultrasonic vibration deposition (Example 1).
[0061] After applying synchronous ultrasonic vibration, the unmelted powder in the molten pool is driven to flow, which increases the powder's absorption of heat from the laser heat source and reduces the chance of defect formation. And by stirring the molten pool, heat exchange is increased, so that the previously solidified deposition layer is heated again, and each two layers are metallurgically bonded again to obtain a denser sample. In addition, due to the effect of acoustic streaming, the flow of the molten pool is enhanced, which will cause the liquid alloy to move to the lower layer and fill the unfused defects. Unfused defects generally exist between two grains, and there is no sufficient metallurgical bonding between layers. After applying synchronous ultrasonic vibration, the unfused defects are eliminated, and only a small amount of pores exist. By reducing unfused defects, the mechanical properties of the laser melt-deposited alloy are improved, and the process window of laser melt-deposited is expanded.
[0062] The mechanical properties of the deposited sample (Comparative Example 1) and the ultrasonic vibration deposited sample (Example 1) in the scanning direction and the deposition direction were compared to analyze the changes in the anisotropy of the mechanical properties.
[0063] Figure 2The stress-strain curves of Ti6Al4V alloys obtained in the deposited state (Comparative Example 1) and ultrasonic vibration assisted laser melting deposition (Example 1). It can be seen that when the tensile stress is along the deposition direction, that is, perpendicular to the direction of the unfused defect, the deposited sample breaks at a stress of about 300MPa. This is because the load is applied along the deposition direction, the long axis of the unfused area is perpendicular to the loading direction, and the stress concentration in the unfused area is high, which provides an easier path for void growth and agglomeration, and breaks at very low stress. When ultrasonic vibration is applied, the unfused defect disappears, leaving only a small amount of spherical pores, which can reduce stress concentration and improve its mechanical properties, basically meeting the performance requirements of forged titanium alloys.
[0064] The plane anisotropy index is used to evaluate the anisotropy of the mechanical properties of different samples, which can be expressed by the following formula:
[0065]
[0066] Where X max and X min Represent the maximum and minimum values of the ultimate tensile strength and elongation, respectively. Table 1 shows the mechanical properties and plane anisotropy index of different samples. For the deposited sample, when the tensile direction is along the deposition direction, that is, the load is perpendicular to the long axis of the unfused defect, the high stress concentration in the unfused defect provides an easier path for the growth and aggregation of the pores. The ultimate tensile strength and elongation of the sample are about 367MPa and 0.27%, respectively. The plane anisotropy index of the ultimate tensile strength and elongation of the deposited sample is about 65.7% and 97.5%, respectively. When ultrasonic vibration is applied, the unfused defect is suppressed, and when stretched along the deposition direction, good strength and plasticity are exhibited. The ultimate tensile strength and elongation plane anisotropy index of the sample drop to 5.6% and 38.1%, respectively.
[0067] Table 1 Mechanical properties and plane anisotropy index of different samples
[0068]
[0069] The present invention is based on laser melting deposition and is assisted by synchronous ultrasonic vibration. The ultrasonic wave can act in the liquid molten pool to produce cavitation and acoustic streaming. It has the advantages that ultrasonic energy is not limited by the height of the sample, the equipment is easy to assemble, and time is saved. It can be applied to the directional energy deposition of titanium alloys, titanium-based composite materials, stainless steel and NiTi alloys and corresponding components in two different ways of wire feeding and powder feeding.
[0070] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. An ultrasonic vibration assisted laser melting deposition additive manufacturing method, characterized in that: The following steps are involved: During the laser melting deposition process, ultrasonic vibration is simultaneously used to ultrasonically treat the laser melting deposition area for additive manufacturing.
2. The additive manufacturing method according to claim 1, characterized in that: The laser power of the laser melting deposition is 1000-2400W; the amplitude of the ultrasonic vibration is 0-100%, and is not 0%.
3. The additive manufacturing method according to claim 1, characterized in that: The material used for the additive manufacturing is titanium alloy, titanium-based composite material, stainless steel or NiTi alloy.
4. The additive manufacturing method according to claim 3, characterized in that: The titanium alloy is Ti6Al4V alloy.
5. The additive manufacturing method according to claim 1, characterized in that: The additive manufacturing is performed using powder or wire.
6. The additive manufacturing method according to claim 5, characterized in that: When powder is used for the additive manufacturing, the powder feeding gas in the laser melting deposition process is argon.
7. The additive manufacturing method according to claim 1, characterized in that: The synchronous use of ultrasonic vibration in the laser melting deposition process specifically includes: moving the ultrasonic impact head and the laser of the laser melting deposition equipment at the same movement speed to perform ultrasonic vibration-assisted laser melting deposition.
8. The additive manufacturing method according to claim 7, characterized in that: The offset distance between the ultrasonic impact head and the laser is 30-80 mm.
9. The additive manufacturing method according to claim 7, characterized in that: The scanning speed during the deposition process was 100-500 mm / min, and the powder feeding rate was 11.2 g / min-19.6 g / min.
10. The material prepared by the additive manufacturing method according to any one of claims 1 to 9.
Citation Information
Cited By
Ultrasonic vibration and powder collection platform for laser additive manufacturing
CN119973146A
An ultrasonic vibration and powder collection platform for laser additive manufacturing
CN119973146B