NiTiLa shape memory alloy and preparation method thereof

By combining Ni, Ti, and La2O3 powders and using 3D printing technology, and optimizing the laser scanning path, the problems of poor forming effect and cracking in NiTi shape memory alloys were solved, enabling the preparation of high-quality NiTiLa shape memory alloys suitable for customized production in the medical field.

CN118926550AInactive Publication Date: 2024-11-12SOUTH CHINA NORMAL UNIV

Patent Information

Application Number
CN202411138426.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing NiTi shape memory alloys have poor forming performance and are prone to cracking, making it difficult to meet the forming requirements of complex irregular components in the medical field.

Method used

Ni, Ti, and La2O3 powders were mixed in a specific ratio, dried, ball-milled, and sieved, and then NiTiLa shape memory alloys were prepared by 3D printing, with layer-by-layer deposition using an optimized laser scanning path.

Benefits of technology

It improves the forming effect of NiTiLa shape memory alloy, reduces the generation of cracks, and is suitable for customized production in the medical field. The process is simple and easy to mass-produce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926550A_ABST
    Figure CN118926550A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of additive manufacturing, and particularly relates to a NiTiLa shape memory alloy and a preparation method thereof.The specific process includes the steps that Ni powder, Ti powder and La2O3 powder are prepared, dried and mixed, and mixed powder is obtained; wherein the mass percent of Ni is 54.51 wt% to 55.51 wt%, the mass percent of Ti is 43.99 wt% to 44.99 wt%, and the mass percent of La2O3 is 0.3 wt% to 0.4 wt%; and the mixed powder is subjected to ball milling refining and screen filtering, and the screened alloy powder is prepared into the NiTiLa shape memory alloy through 3D printing. According to the method, the high-quality NiTiLa shape memory alloy which is good in forming effect and not prone to crack generation is obtained, the method can be applied to exclusive customized production in the medical field, the process is simple and clear, operability is high, and large-scale production is easy to achieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of additive manufacturing, and in particular relates to a NiTiLa shape memory alloy and a preparation method thereof. Background Art

[0002] In recent years, laser selective melting additive manufacturing (SLM) technology has developed rapidly. Based on the complete melting mechanism and the characteristics of micro-refined layer-by-layer processing, this technology has unique advantages in the high-performance precision forming of parts with complex configurations. In addition, this technology has the advantages of flexibility, easy to realize intelligence, short production cycle, and the ability to produce parts with very high mechanical properties. It is widely used in national defense, medical, metallurgy and other fields.

[0003] Among shape memory alloys, NiTi series alloys have the characteristics of high strength, high toughness and high biocompatibility and are widely used in the medical field.

[0004] Due to the exclusive customized production in the medical field and the forming and preparation of complex special-shaped components in the medical field, it is difficult to obtain good forming quality by casting. The preparation of NiTi shape memory alloy by selective laser melting has become a hot topic in the field of additive manufacturing. However, the currently prepared NiTi shape memory alloy has poor forming effect and is prone to cracks. Therefore, there is an urgent need to develop a new type of NiTi shape memory alloy. Summary of the invention

[0005] The invention provides a NiTiLa shape memory alloy and a preparation method thereof, so as to solve the problems in the prior art that the NiTi shape memory alloy has poor forming effect and is prone to cracking.

[0006] To achieve the above object, the present invention proposes the following technical solutions: A method for preparing a NiTiLa shape memory alloy comprises the following steps: Step 1, preparing powders of Ni, Ti and La2O3, drying and mixing them to obtain mixed powder; The mass percentage of Ni is 54.51-55.51wt.%, the mass percentage of Ti is 43.99-44.99wt.%, and the mass percentage of La2O3 is 0.3-0.4wt.%; Step 2, ball-milling the mixed powder to obtain alloy powder; Step 3, filtering the alloy powder through a sieve to obtain screened alloy powder; Step 4: The screened alloy powder is 3D printed to make NiTiLa shape memory alloy.

[0007] Preferably, the particle size of the Ni, Ti, and La2O3 powders is 15-53 μm.

[0008] Preferably, in step 1, the three powders of Ni, Ti and La2O3 are mixed in a ratio of 55.51wt.%, 43.99wt.%, and 0.3wt.%.

[0009] Preferably, the drying in step 1 is specifically as follows: Place Ni, Ti and La2O3 powders in a drying oven at a drying temperature of 70-80°C for 2-3 hours.

[0010] Preferably, in step 2, the ball milling treatment is specifically as follows: The ball milling speed was 200 r / min, the ball milling time was 10 h, the ball milling mode was alternating clockwise and counterclockwise rotation, and the single rotation time was 30 min.

[0011] Preferably, in step 2, in the ball milling refinement treatment, the ball milling balls used are zirconium oxide grinding balls with a particle size of 1 mm, and the ball-powder ratio of the grinding balls to the mixed powder is 19-21:1.

[0012] Preferably, the specific process of the 3D printing is: Establish a three-dimensional model of the specimen; The three-dimensional model is sliced ​​and sliced ​​to obtain a sliced ​​model; Import the sliced ​​model into the 3D printer; Based on the slicing model, the screened alloy powder and reverse 3D printing were used to make NiTiLa shape memory alloy.

[0013] Preferably, the 8*8*8 cube of the three-dimensional model has a slice thickness of 0.03 mm.

[0014] Preferably, the laser scanning path used in the 3D printing process is: The processing sample is divided into the smallest unit of 5*5mm, and the laser beam moves in an S shape along the x-axis.

[0015] A NiTiLa shape memory alloy is prepared by the NiTiLa shape memory alloy preparation method.

[0016] The present invention is beneficial in that: The present invention proposes to mix three kinds of powders of Ni, Ti and La2O3 in proportion, and put them into 3D printing after drying, ball milling and sieving for production, so as to obtain high-quality NiTiLa shape memory alloy with good molding effect and not prone to cracks. The alloy can be applied to exclusive customized production in the medical field, and the process is simple and clear, the operability is strong, and it is easy to put into large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings: Figure 1 A method for preparing a NiTiLa shape memory alloy; Figure 2 Schematic diagram of the laser movement path of 3D printing during the preparation of NiTiLa shape memory alloy; Figure 3 A schematic diagram of a NiTiLa shape memory alloy; Figure 4 The invention is a memory alloy prepared by the prior art. DETAILED DESCRIPTION

[0018] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0019] The following detailed description is an exemplary description, which is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.

[0020] See also Figure 1 As shown, the present invention provides a method for preparing a NiTiLa shape memory alloy, comprising the following steps: Step 1, preparing Ni, Ti, and La2O3 powders, wherein the particle size of the Ni, Ti, and La2O3 powders is 15-53 μm, and drying the Ni, Ti, and La2O3 powders; Step 2, mixing Ni, Ti and La2O3 powders to obtain mixed powder; The mass percentage of Ni is 54.51-55.51wt.%, the mass percentage of Ti is 43.99-44.99wt.%, and the mass percentage of La2O3 is 0.3-0.4wt.%; Step 3, ball-milling the mixed powder to obtain alloy powder; The particle size of the ball milling ball is 1 mm, the material is zirconium oxide, the ball-to-powder ratio is 19-21:1, the ball milling speed is 200 r / min, the ball milling time is 10 h, the ball milling mode is clockwise and counterclockwise alternating rotation, and the single rotation time is 30 min; Step 4, filtering the alloy powder obtained in step 3 through a sieve to obtain screened alloy powder.

[0021] Step 5: Print the NiTiLa shape memory alloy layer by layer using 3D printing. Specifically: Establish a three-dimensional model of the sample, and the three-dimensional model can be selected differently according to specific needs; The three-dimensional model is sliced ​​and sliced ​​to obtain a sliced ​​model; Import the sliced ​​model into the 3D printer; The screened alloy powder is pretreated and 3D printed. The laser scanning strategy used in the 3D printing process includes: dividing the processing sample into the smallest unit of 5*5mm, and the laser beam moves in an S-shape along the x-axis, which effectively reduces the heat accumulation of the laser scanning in the scanning area, and effectively dissipates the residual heat while ensuring good metallurgical bonding of the molten pool to avoid heat accumulation. Figure 2 shown.

[0022] In a specific embodiment, the drying process in step 1 is: placing Ni, Ti, and La2O3 powders in a drying oven, with a drying temperature of 70 to 80°C and a drying time of 2 to 3 hours.

[0023] In a specific embodiment, the 200-mesh screen is used to sieve the alloy powder.

[0024] In a specific embodiment, the three-dimensional model is a cube of 8*8*8, and the slice thickness is 0.03 mm. In a specific embodiment, the pretreatment process is to dry the screened alloy powder at a temperature of 70 to 80° C. for 2 to 3 hours.

[0025] A method for preparing a NiTiLa shape memory alloy is specifically as follows: Step 1, preparing Ni, Ti, and La2O3 powders, and placing the Ni, Ti, and La2O3 powders in a drying oven for drying; Step 2, mixing Ni, Ti, and La2O3 powders in a ratio of 55.51wt.%, 43.99wt.%, and 0.3wt.% to obtain a mixed powder; Step 3, ball-milling the mixed powder to obtain alloy powder; The ball milling balls were zirconia balls with a particle size of 1 mm, the ball-to-powder ratio was 20:1, the ball milling speed was 200 r / min, the ball milling time was 10 h, the ball milling mode was alternating clockwise and counterclockwise rotation, and the single rotation time was 30 min; Step 4, filtering the alloy powder obtained in step 3 through a 200-mesh sieve to obtain screened alloy powder.

[0026] Step 5: Print the NiTiLa shape memory alloy layer by layer using 3D printing. Specifically: Establish a three-dimensional model of the sample, the three-dimensional model is an 8*8*8 cube, and slice the three-dimensional model in layers with a slice thickness of 0.03 mm to obtain a sliced ​​model; The sliced ​​model was imported into the 3D printer, and the screened alloy powder was dried at 80°C for 2 h and imported into the 3D printer; The 3D printer prints the sliced ​​model to obtain the finished product, such as Figure 3 shown.

[0027] The present invention also provides a NiTiLa shape memory alloy, wherein the NiTiLa shape memory alloy is prepared by the above-mentioned NiTiLa shape memory alloy preparation method.

[0028] The NiTiLa shape memory alloy provided by the present invention is compared Figure 4 The memory alloy prepared by the prior art shown in the figure does not involve the La element. It can be seen that compared with the finished product prepared by the method described in the present invention, the memory alloy prepared by the prior art has poor forming effect and cracks. The preparation method proposed in the present invention has good forming effect, and the cracks and thermal deformation of the finished product are reduced.

[0029] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.

[0030] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a NiTiLa shape memory alloy, It is characterized in that The steps include: Step 1, preparing powders of Ni, Ti and La2O3, drying and mixing them to obtain mixed powder; The mass percentage of Ni is 54.51-55.51wt.%, the mass percentage of Ti is 43.99-44.99wt.%, and the mass percentage of La2O3 is 0.3-0.4wt.%; Step 2, ball-milling the mixed powder to obtain alloy powder; Step 3, filtering the alloy powder through a sieve to obtain screened alloy powder; Step 4: The screened alloy powder is 3D printed to make NiTiLa shape memory alloy.

2. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that The particle size of Ni, Ti and La2O3 powders is 15-53 μm.

3. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that In step 1, Ni, Ti, La 2 O 3 The three powders were mixed in a ratio of 55.51wt.%, 43.99wt.%, and 0.3wt.%.

4. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that The drying in step 1 is specifically as follows: Place Ni, Ti and La2O3 powders in a drying oven at a drying temperature of 70-80°C for 2-3 hours.

5. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that In step 2, the ball milling treatment is specifically as follows: The ball milling speed was 200 r / min, the ball milling time was 10 h, the ball milling mode was alternating clockwise and counterclockwise rotation, and the single rotation time was 30 min.

6. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that In step 2, in the ball milling refinement treatment, the ball milling balls used are zirconium oxide grinding balls with a particle size of 1 mm, and the ball-powder ratio of the grinding balls to the mixed powder is 19-21:

1.

7. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that The specific process of 3D printing is as follows: Establish a three-dimensional model of the specimen; The three-dimensional model is sliced ​​and sliced ​​to obtain a sliced ​​model; Import the sliced ​​model into the 3D printer; Based on the slicing model, the screened alloy powder and reverse 3D printing were used to make NiTiLa shape memory alloy.

8. A method for preparing a NiTiLa shape memory alloy as claimed in claim 7, It is characterized in that The 8*8*8 cube of the three-dimensional model has a slice thickness of 0.03 mm.

9. A method for preparing a NiTiLa shape memory alloy as claimed in claim 1, It is characterized in that The laser scanning path used in the 3D printing process is: The processing sample is divided into the smallest unit of 5*5mm, and the laser beam moves in an S shape along the x-axis.

10. A NiTiLa shape memory alloy, It is characterized in that The NiTiLa shape memory alloy is prepared by a NiTiLa shape memory alloy preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Rare earth modified laser cladding layer and preparation process thereof

    CN106756996A

  • Method for improving high and low temperature mechanical and corrosion performance of conventional alloy based on grain boundary bonding and in-situ reaction

    CN117867311A

  • Wear-resistant titanium alloy and additive preparation method thereof

    CN118086721A

  • High-strength wear-resistant antioxidant titanium-based composite material and preparation method thereof

    CN118109718A

  • Nano-lanthanum oxide reinforced tungsten-based composite material and preparation method thereof

    US20230101137A1

Cited By

  • Additive manufacturing high-phase-change-temperature high-elongation nickel-titanium alloy and preparation method and application thereof

    CN121178875A