Method for improving magnesium / aluminum alloy ultrathin plate joint performance

By clamping the intermediate layer of zinc foil and nickel foil in the joint area of ​​magnesium alloy and aluminum alloy ultra-thin plates, and using nanosecond pulsed laser welding, the defects and metallurgical incompatibility problems in welding of magnesium alloy and aluminum alloy are solved. Significantly improves the mechanical properties and welding quality of the joints.

CN118926700APending Publication Date: 2024-11-12NORTHEAST FORESTRY UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411250708.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the welding process, magnesium alloys and aluminum alloys are prone to defects such as pores and cracks, and due to metallurgical incompatibility, hard and brittle intermetallic compounds are generated at the interface, resulting in unsatisfactory joint performance. Conventional welding methods cannot guarantee uniform longitudinal energy. Input leads to a large temperature gradient and affects the mechanical properties.

Method used

Zinc foil and nickel foil are clamped as intermediate layers in the overlap area of ​​magnesium alloy ultra-thin plate and aluminum alloy ultra-thin plate, and laser welding is performed using nanosecond pulsed laser emitter. The process parameters are laser power 20W~50W and welding speed 10mm/s~70mm/s, pulse frequency 20kHz~30kHz, welded according to the concentric laser scanning path.

Benefits of technology

The zinc foil-nickel foil intermediate layer absorbs laser energy to control the temperature, blocks the flow of liquid metal, avoids mixing of Mg-Al elements, and generates a tough phase, significantly improves the mechanical properties of magnesium/aluminum alloy ultra-thin plate joints, reduces defects, and improves the temperature gradient Distribution to improve welding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926700A_ABST
    Figure CN118926700A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the performance of a magnesium / aluminum alloy ultra-thin plate joint, which comprises the following steps of: lapping a pretreated aluminum alloy ultra-thin plate and a pretreated magnesium alloy ultra-thin plate, arranging the aluminum alloy ultra-thin plate at the upper part and the magnesium alloy ultra-thin plate at the lower part, clamping a middle layer in a lapping area, and sequentially arranging zinc foil and nickel foil on the middle layer from top to bottom to obtain a to-be-welded part; and laser welding is conducted on the lap joint area of the to-be-welded part. According to the method, the thermal defect caused by too high magnesium alloy temperature due to too high laser energy can be effectively controlled, the welding seam forming quality is better, the joint defect is fewer, the element diffusion phenomenon can be inhibited, a ductile phase replaces a brittle phase, the metallurgical reaction occurring in a molten pool is improved, and the welding quality is improved. And the mechanical property of the magnesium / aluminum alloy ultrathin plate joint is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding technology for dissimilar metal materials, and in particular relates to a method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints. Background Art

[0002] Magnesium alloys have the characteristics of low density, high specific strength, and high plasticity, while aluminum alloys have the characteristics of low cost and strong corrosion resistance. Mg / Al composite structural material components can combine the advantages of both and have good adaptability to the needs of high-quality development of the manufacturing industry. They can be widely used in aerospace, transportation and other fields, and have broad application prospects. Therefore, the successful connection of magnesium alloys and aluminum alloys has become an inevitable trend of future development.

[0003] However, as two dissimilar metals, magnesium alloy and aluminum alloy have great differences in thermophysical properties, such as boiling point difference (magnesium alloy is about 1380K, aluminum alloy is about 2793K), thermal conductivity difference (magnesium alloy is about 114W·m -1 ·k -1 、Aluminum alloy is about 167W·m -1 ·k -1 ), etc. The existence of these differences makes it very easy to have defects such as pores and cracks during the magnesium / aluminum connection process, and due to metallurgical incompatibility, it is very easy to produce hard and brittle Mg-Al intermetallic compounds (IMC) at the magnesium / aluminum interface, including Mg 17 Al 12 , Mg2Al3 and MgAl, which makes the performance of the joint obtained after the magnesium / aluminum alloy is not ideal. In addition, when the conventional welding method is used to weld the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate, it is usually impossible to ensure that the laser heat source can have a balanced longitudinal energy input inside the joint, which leads to a large temperature gradient in the longitudinal direction inside the joint, so that the upper IMC layer is thick and the bottom is even not fused, which seriously affects the mechanical properties of the joint. Therefore, how to overcome the above defects and obtain a method to improve the performance of magnesium / aluminum alloy ultra-thin plate joints is of great significance for realizing the widespread application of magnesium / aluminum alloy ultra-thin plate connectors. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions.

[0006] A method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints, comprising the following steps:

[0007] S1. Pre-treating the aluminum alloy ultra-thin plate and the magnesium alloy ultra-thin plate;

[0008] S2, overlapping a pretreated aluminum alloy ultra-thin plate and a pretreated magnesium alloy ultra-thin plate, and sandwiching an intermediate layer in the overlapping area to obtain a weldment; the pretreated aluminum alloy ultra-thin plate is on the top, the pretreated magnesium alloy ultra-thin plate is on the bottom, and the intermediate layers are zinc foil and nickel foil from top to bottom;

[0009] S3. Laser welding is performed on the overlapping areas of the workpieces to be welded.

[0010] The above method is further improved, in step S2, the thickness of the zinc foil is 0.01 mm to 0.03 mm, and the purity of the zinc foil is ≥ 99.9%; the thickness of the nickel foil is 0.01 mm to 0.03 mm, and the purity of the nickel foil is ≥ 99.9%.

[0011] The above method is further improved, in step S1, the thickness of the magnesium alloy ultra-thin plate is 0.1 mm to 0.5 mm, and the thickness of the aluminum alloy ultra-thin plate is 0.1 mm to 0.5 mm.

[0012] The above method is further improved in that the widths of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate are the same; the size and shape of the nickel foil and the zinc foil are the same and can completely cover the overlapping area.

[0013] The above method is further improved in that in step S3, the laser welding is performed using a nanosecond pulse laser emitter.

[0014] The above method is further improved, in step S3, the process parameters of the laser welding are: laser power of 20W to 50W, welding speed of 10mm / s to 70mm / s, pulse frequency of 20kHz to 30kHz, and defocus of 0.

[0015] The above method is further improved, in step S3, the laser welding is performed according to a concentric circle laser scanning path; the concentric circle laser scanning path is specifically: the diameter of the outermost circle of the preset concentric circles is 3.6 mm, the diameter of the innermost circle is 0.08 mm, and the diameter of each adjacent concentric circle differs by 0.08 mm, and the laser beam of the laser welding equipment is moved along the gap between adjacent concentric circles to form a concentric circle welding trajectory from the outside to the inside.

[0016] The above method is further improved, in step S3, the maximum output power of the nanosecond pulse laser emitter is 50W, the pulse frequency is 20kHz to 200kHz, and the spot diameter is 0.1mm.

[0017] The above method is further improved, in step S3, the workpiece to be welded is first subjected to the following treatment before laser welding: the workpiece to be welded is clamped with a clamp; the gap between the materials of the workpiece to be welded is less than 0.1 mm.

[0018] The above method is further improved, in step S1, the pretreatment is grinding, polishing, soaking and drying in sequence; the specific process of the grinding is: using 400 mesh, 800 mesh and 1200 mesh sandpaper to grind the surface of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate respectively; the specific process of polishing is: polishing the ground magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate respectively, and adding diamond spray polishing agent during the polishing process; the polishing is performed by a polishing machine, the rotation speed of the polishing machine is 300r / min, and the particle size of the diamond spray polishing agent is 2.5μm; the soaking is soaking in anhydrous ethanol; the drying is blown dry by a cold air blower.

[0019] The above method is further improved, in which in step S1, the material of the aluminum alloy ultra-thin plate is 6061 aluminum alloy, and the material of the magnesium alloy ultra-thin plate is AZ31B magnesium alloy.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] (1) The present invention provides a method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints. The aluminum alloy ultra-thin plate is placed on the top and the magnesium alloy ultra-thin plate is placed on the bottom. The two are overlapped, and zinc foil-nickel foil is embedded in the overlap area as an intermediate layer for laser welding. The method of the present invention uses zinc foil-nickel foil as an intermediate layer. On the one hand, it can absorb part of the laser energy and effectively control the thermal defects caused by the excessive temperature of the magnesium alloy due to excessive laser energy, so that the weld forming quality is better and the joint defects are less; on the other hand, it can block the direct contact caused by the flow of liquid magnesium / aluminum during laser welding, thereby curbing the mixing of Mg and Al elements, effectively avoiding the formation of brittle Mg-Al intermetallic compounds, and at the same time, a large amount of mixed toughness phases such as Mg-Zn, Mg-Ni and Al-Ni are generated at the joint surface, so that the mechanical properties of the magnesium / aluminum alloy ultra-thin plate joint are greatly improved. The method of the present invention can be widely used in the fields related to the laser welding of magnesium alloy ultra-thin plates and aluminum alloy ultra-thin plates. The thickness of the magnesium alloy ultra-thin plates and aluminum alloy ultra-thin plates can be as low as 0.2 mm, and the application prospects are very broad.

[0022] (2) The method of the present invention uses a nanosecond pulse laser emitter for laser welding. The process parameters of laser welding are: laser power of 20W to 50W, welding speed of 10mm / s to 70mm / s, pulse frequency of 20kHz to 30kHz, defocus of 0, and a concentric laser scanning path. The distribution of the laser temperature field can be improved, which is beneficial to reducing the temperature gradient inside the joint and regulating a more uniform laser energy field in the longitudinal direction of the joint, so that the forming quality of the magnesium / aluminum alloy ultra-thin plate joint is better and the phenomenon of insufficient welding is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the workpiece to be welded being clamped on a welding workbench in Example 1 of the present invention.

[0024] Figure 2 It is a schematic diagram of overlapping the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in Example 1 of the present invention.

[0025] Figure 3 Schematic diagram of the laser scanning path of laser welding in Example 1 of the present invention.

[0026] Figure 4 This is a physical picture of the surface of the weld after laser welding of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in Example 1 of the present invention. Figure 4 In the figure, (a) is the weld on the aluminum side, and (b) is the weld on the magnesium side.

[0027] Figure 5 This is a physical picture of the surface of the weld after laser welding of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in Comparative Example 1. Figure 5 In the figure, (a) is the weld on the aluminum side, and (b) is the weld on the magnesium side.

[0028] Figure 6 The SEM images of the molten pools after welding the ultra-thin magnesium alloy plates and the ultra-thin aluminum alloy plates in Example 1 and Comparative Examples 1-4 of the present invention are shown. Figure 6 Among them, (a) is the SEM image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in comparison example 1, (b) is the SEM image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in comparison example 2, (c) is the SEM image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in comparison example 3, (d) is the SEM image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in comparison example 4, and (e) is the SEM image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in embodiment 1.

[0029] Figure 7 This is an EDS image of the molten pool after welding the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in Example 1 of the present invention and Comparative Example 1. Figure 7In the figure, (a) is the EDS image of the molten pool after welding the ultra-thin magnesium alloy plate and the ultra-thin aluminum alloy plate in comparative example 1, and (b) is the EDS image of the molten pool after welding the ultra-thin magnesium alloy plate and the ultra-thin aluminum alloy plate in embodiment 1.

[0030] Figure 8 1 and 2 are XRD diagrams of the welded joints of the magnesium alloy ultra-thin plates and the aluminum alloy ultra-thin plates in Example 1 and Comparative Example 1 of the present invention. Figure 8 In the figure, (a) is the XRD diagram of the welded joint of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in comparative example 1, and (b) is the XRD diagram of the welded joint of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate in embodiment 1.

[0031] Fig. 9 It is a histogram of the tensile strength of the welded joints of the magnesium alloy ultra-thin plates and the aluminum alloy ultra-thin plates in Example 1 and Comparative Examples 1-4 of the present invention.

[0032] Fig.10 It is a histogram of the tensile strength of the welded joints of the magnesium alloy ultra-thin plates and the aluminum alloy ultra-thin plates in Example 1 and Comparative Examples 5 to 7 of the present invention.

[0033] The symbols in the figure represent:

[0034] 1. Ultra-thin magnesium alloy plate; 2. Ultra-thin aluminum alloy plate; 3. Clamp; 4. Bolt; 5. Welding area; 6. Workbench; 7. Bolt hole; 8. Intermediate layer; 9. Pulse laser. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.

[0036] Embodiment 1:

[0037] A method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints of the present invention comprises the following steps:

[0038] S1. AZ31B magnesium alloy ultra-thin plate, 6061 aluminum alloy ultra-thin plate, nickel foil and zinc foil are selected as raw materials. The size specifications of magnesium alloy ultra-thin plate and aluminum alloy ultra-thin plate are 50mm×10mm×0.2mm, the size specifications of nickel foil and zinc foil are 10mm×10mm×0.02mm, and the purity of zinc foil and nickel foil are both 99.9%.

[0039] (2) The surfaces of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate were polished with sandpaper of 400 mesh, 800 mesh, and 1200 mesh, respectively, to remove surface oxides; then, a polishing disc with a rotation speed of 300 r / min was used for polishing, and a diamond spray polishing agent with a particle size of 2.5 μm was added during the polishing process to increase the friction of the polishing cloth to remove surface scratches; the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate were immersed in anhydrous ethanol for five minutes, and dried with a cold air blower; and a pretreated magnesium alloy ultra-thin plate and a pretreated aluminum alloy ultra-thin plate were obtained.

[0040] (3) The pretreated aluminum alloy ultra-thin plate is placed on the top and the pretreated magnesium alloy ultra-thin plate is placed on the bottom. The two are overlapped, and zinc foil and nickel foil are embedded in the overlap area from top to bottom as the middle layer. The overlapped area is clamped on the welding workbench with a clamp, such as Figure 1 , Figure 2 As shown, the welded parts are obtained; that is, the welded parts are pretreated aluminum alloy ultra-thin plate, zinc foil, nickel foil, and pretreated magnesium alloy ultra-thin plate from top to bottom, and the gap between the materials of the welded parts is less than 0.1 mm.

[0041] Specific operation: overlap the pretreated materials on the workbench 6 in the order of overlapping from top to bottom: aluminum alloy ultra-thin plate 2, middle layer 8, magnesium alloy ultra-thin plate 1, then press the clamp 3 on the overlapped workpiece, pass the bolt 4 through the clamp 3 and tighten it in the bolt hole 7, fix the workpiece on the workbench 6, and expose the welding area 5; then, adjust the laser welding parameters, draw the laser scanning path, and emit the pulse laser 9 for nanosecond pulse laser welding.

[0042] (4) Using a nanosecond pulse laser emitter to perform laser welding on the overlapped area of ​​the workpiece to be welded; wherein the laser welding is performed according to a concentric laser scanning path, such as Figure 3 As shown, specifically: the outermost diameter of the preset concentric circles is 3.6mm, the innermost diameter is 0.08mm, the diameter difference between each two adjacent circles is 0.08mm, and the circular ring with a spacing of 0.04mm between two adjacent circles is used as the welding pattern, and welding is performed from the outside to the inside, that is, moving from the outermost concentric circle to the innermost concentric circle; the process parameters of laser welding are: laser power is 25W, laser scanning speed is 50mm / s, pulse frequency is 20kHz, and defocus is 0.

[0043] In this embodiment, the nanosecond pulse laser transmitter used is a JW-F30W laser, the maximum output power of the laser is 50W, the pulse frequency is 20kHz to 200kHz, and the spot diameter is 0.1mm.

[0044] Table 1 Composition of AZ31B magnesium alloy ultra-thin plate (mass percentage)

[0045] Mg Al Zn Mn Si Fe Cu Ni >95 3.1 0.9 0.32 0.012 0.0021 0.009 0.0009

[0046] Table 2 Composition of 6061 aluminum alloy ultra-thin plate (mass percentage)

[0047] Al Mg Mn Si Fe Cu Cr Zn Ti >96 0.6~1.2 0.15 0.40 0.70 0.15 0.05~0.35 0.25 0.1

[0048] Comparative Example 1:

[0049] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), no intermediate layer is provided in the overlapping area.

[0050] Comparative Example 2:

[0051] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), only zinc foil is embedded in the overlap area as an intermediate layer.

[0052] Comparative Example 3:

[0053] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), only titanium foil is embedded in the overlap area as an intermediate layer.

[0054] Comparative Example 4:

[0055] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), only nickel foil is embedded in the overlap area as an intermediate layer.

[0056] Comparative Example 5:

[0057] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), titanium foil and zinc foil are embedded in the overlap area from top to bottom as intermediate layers.

[0058] Comparative Example 6:

[0059] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), nickel foil and zinc foil are embedded in the overlap area from top to bottom as an intermediate layer.

[0060] Comparative Example 7:

[0061] A method for welding magnesium / aluminum alloy ultra-thin plates is basically the same as the method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints in Example 1, with the only difference being that in step (3), nickel foil and titanium foil are embedded in the overlap area from top to bottom as intermediate layers.

[0062] The microstructure of the weld was observed by SEM scanning electron microscope; the element distribution at the cross section was observed by EDS quantitative dispersion spectrometer; the phase composition of the joint was detected by X-ray diffractometer; the tensile test of the welded joint was carried out by universal testing machine at room temperature, and the average value of three data points was taken. The results are as follows Figures 4 to 10 shown.

[0063] Combination Figure 4 , Figure 5 It can be seen that in Comparative Example 1, when the aluminum alloy ultra-thin plate and the magnesium alloy ultra-thin plate were welded without adding an intermediate layer, cracks of varying degrees were generated in the middle and edge of the aluminum side weld, and the magnesium side showed a clear weld with cracks in the center. Compared with Comparative Example 1, in Example 1, the aluminum alloy ultra-thin plate and the magnesium alloy ultra-thin plate were laser welded with zinc foil-nickel foil as the intermediate layer, and the aluminum side had good formability, the magnesium side weld was blurred, and no weld appeared in the center, showing a good temperature distribution, avoiding the thermal defects of the magnesium alloy at high temperature. It can be seen that the method of the present invention uses zinc foil-nickel foil as the intermediate layer, and can absorb part of the laser energy when laser welding the aluminum alloy ultra-thin plate and the magnesium alloy ultra-thin plate, effectively controlling the thermal defects caused by the excessive temperature of the magnesium alloy due to the excessive laser energy, so that the weld formation quality is better and the joint defects are less.

[0064] Combination Figure 6 to Figure 8 It can be seen that in Comparative Example 1, without adding an intermediate layer, the diffusion of Mg and Al elements is strong, producing Mg 17 Al 12, Mg2 Al3 and other binary brittle phases. In Comparative Example 2, zinc foil is used as the intermediate layer. As shown in Figure (b), due to the low boiling point of zinc foil, it vaporizes under the irradiation of high-energy laser beam, and the existence of the intermediate layer can no longer be observed in the SEM image. It can be seen that the inhibitory effect of zinc foil as an intermediate layer on the diffusion of Mg and Al elements is not obvious. In Comparative Example 3, titanium foil is used as the intermediate layer. As shown in Figure (c), under the action of pulsed laser, titanium foil appears in the intermediate layer area as a "slim strip", and the distance between the two pulse points is large. Since the titanium foil is not fully melted to form liquid metal (the melting point of titanium is 1933K), it is impossible to inhibit the combination of Mg and Al elements. In Comparative Example 4, nickel foil is used as the intermediate layer. As shown in Figure (d), although it can be seen that the nickel foil has been fully melted to form liquid metal, there is an obvious and large collapse, which is not conducive to the improvement of the mechanical properties of the joint. Compared with no intermediate layer, zinc foil intermediate layer, titanium foil intermediate layer, and nickel foil intermediate layer, in Example 1, zinc foil-nickel foil is used as the intermediate layer. Under the action of high energy density of pulsed laser, zinc foil and nickel foil effectively inhibit the diffusion between Mg and Al elements, and instead produce binary toughness phases such as MgZn2, MgZn, AlNi3, AlNi, and MgNi2 at the bonding surface, thereby improving the mechanical properties of the welded joint; at the same time, Mg-Al-Zn ternary toughness phase is produced at the bonding surface, further improving the mechanical properties of the welded joint. It can be seen that in the present invention, zinc foil-nickel foil is used as the intermediate layer to perform laser welding on aluminum alloy ultra-thin plates and magnesium alloy ultra-thin plates, which can not only effectively block the deep diffusion of Mg and Al elements at the bonding surface, but also produce a large amount of mixed toughness phases such as Mg-Zn, Mg-Ni and Al-Ni, making the Mg-Al brittle phase controllable, thereby improving the mechanical properties and corrosion resistance of the welded joint.

[0065] Combination Fig. 9 , Fig.10 It can be seen that compared with the comparative example 1 in which no intermediate layer is added, the tensile strength of the welded joint using zinc foil, titanium foil, nickel foil, and nickel foil-zinc foil as the intermediate layer is improved very limitedly; while the tensile strength of the welded joint using titanium foil-zinc foil and nickel foil-titanium foil as the intermediate layer is decreased; in Example 1, zinc foil-nickel foil is used as the intermediate layer, and the tensile strength of the welded joint reaches 70.2 MPa, an increase of 26.5%.

[0066] In summary, the method of the present invention uses zinc foil-nickel foil as the intermediate layer. On the one hand, it improves the surface morphology of the weld, makes the temperature distribution inside the joint more uniform, and effectively controls the excessive generation of thermal defects; on the other hand, it inhibits the occurrence of element diffusion, replaces the brittle phase with the tough phase, improves the metallurgical reaction inside the molten pool, and greatly improves the mechanical properties of the welded joint. The method of the present invention is suitable for the fields related to laser welding of magnesium / aluminum alloy ultra-thin plates, such as nanosecond pulse laser welding, and has a wide range of application prospects.

[0067] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints, It is characterized in that The following steps are involved: S1. Pre-treating the aluminum alloy ultra-thin plate and the magnesium alloy ultra-thin plate; S2, overlapping a pretreated aluminum alloy ultra-thin plate and a pretreated magnesium alloy ultra-thin plate, and sandwiching an intermediate layer in the overlapping area to obtain a weldment; the pretreated aluminum alloy ultra-thin plate is on the top, the pretreated magnesium alloy ultra-thin plate is on the bottom, and the intermediate layers are zinc foil and nickel foil from top to bottom; S3. Laser welding is performed on the overlapping areas of the workpieces to be welded.

2. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to claim 1, It is characterized in that In step S2, the thickness of the zinc foil is 0.01 mm to 0.03 mm, and the purity of the zinc foil is ≥ 99.9%. The thickness of the nickel foil is 0.01 mm to 0.03 mm, and the purity of the nickel foil is ≥ 99.9%.

3. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to claim 2, It is characterized in that In step S1, the thickness of the magnesium alloy ultra-thin plate is 0.1 mm to 0.5 mm, and the thickness of the aluminum alloy ultra-thin plate is 0.1 mm to 0.5 mm.

4. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to any one of claims 1 to 3, It is characterized in that In step S3, the laser welding is performed using a nanosecond pulse laser emitter.

5. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to claim 4, It is characterized in that In step S3, the process parameters of the laser welding are: laser power of 20W to 50W, welding speed of 10mm / s to 70mm / s, pulse frequency of 20kHz to 30kHz, and defocus of 0.

6. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to claim 5, It is characterized in that In step S3, the laser welding is performed according to a concentric circle laser scanning path; the concentric circle laser scanning path is specifically as follows: the diameter of the outermost circle of the preset concentric circle is 3.6 mm, the diameter of the innermost circle is 0.08 mm, and the diameters of each adjacent concentric circle differ by 0.08 mm. The laser beam of the laser welding equipment is moved along the gap between adjacent concentric circles to form a concentric circle welding trajectory from the outside to the inside.

7. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to claim 6, It is characterized in that In step S3, the maximum output power of the nanosecond pulse laser emitter is 50 W, the pulse frequency is 20 kHz to 200 kHz, and the spot diameter is 0.1 mm.

8. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to any one of claims 1 to 3, It is characterized in that In step S3, the workpiece to be welded is first processed as follows before laser welding: the workpiece to be welded is clamped by a clamp; and the gap between the materials of the workpiece to be welded is less than 0.1 mm.

9. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to any one of claims 1 to 3, It is characterized in that In step S1, the pretreatment is grinding, polishing, soaking and drying in sequence; the specific process of the grinding is: using 400 mesh, 800 mesh and 1200 mesh sandpaper to grind the surface of the magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate respectively; the specific process of polishing is: polishing the ground magnesium alloy ultra-thin plate and the aluminum alloy ultra-thin plate respectively, and adding diamond spray polishing agent during the polishing process; the polishing is performed by a polishing machine, the rotation speed of the polishing machine is 300r / min, and the particle size of the diamond spray polishing agent is 2.5μm; the soaking is soaking in anhydrous ethanol; the drying is blown dry by a cold air blower.

10. The method for improving the performance of magnesium / aluminum alloy ultra-thin plate joints according to any one of claims 1 to 3, It is characterized in that In step S1, the material of the aluminum alloy ultra-thin plate is 6061 aluminum alloy, and the material of the magnesium alloy ultra-thin plate is AZ31B magnesium alloy.

Citation Information

Cited By

  • Welding method for aluminum-magnesium dissimilar alloy and application of welding method

    CN119794569A