Method for reducing large particles on surface of silicon wafer before single-side grinding, grinding method and silicon wafer

Through ultrasonic cleaning of cleaning liquid, cleaning liquid cleaning, moisturizing liquid cleaning and electrostatic elimination device, the problem of large particles on the surface of the silicon wafer before single-sided grinding is solved, and the yield and grinding accuracy of the silicon wafer are improved.

CN118927028APending Publication Date: 2024-11-12SHANGHAI ADVANCED SILICON TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410997504.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has problems of incomplete cleaning and large particles in reducing the surface of silicon wafers before single-sided grinding, resulting in a low yield rate of silicon wafers.

Method used

Using the combination of ultrasonic cleaning of cleaning liquid, cleaning liquid cleaning, moisturizing liquid cleaning and slow lifting and drying in the electrostatic elimination device, the charge on the surface of the silicon wafer is initially washed and neutralized, to avoid adhesion of large particles and ensure the surface of the silicon wafer. cleanliness.

Benefits of technology

The yield rate after single-sided grinding of silicon wafers is significantly improved, ensuring the cleanliness of the silicon wafer surface, reducing large particles adsorption, and improving the accuracy and production capacity of the grinding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927028A_ABST
    Figure CN118927028A_ABST
Patent Text Reader

Abstract

The invention provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, a grinding method and the silicon wafer. The method comprises the following steps: cleaning the silicon wafer before single-side grinding; the cleaning step comprises cleaning fluid ultrasonic cleaning, cleaning fluid cleaning, moisturizing fluid cleaning and slow lifting drying which are carried out in sequence, and the slow lifting drying is carried out in an electrostatic elimination device. According to the method provided by the invention, primary cleaning of large particles adsorbed on the surface of the silicon wafer is realized through ultrasonic cleaning of the cleaning liquid; cleaning of large particles stained on the surface of the silicon wafer is further achieved through cleaning of the cleaning liquid and cleaning of the moisturizing liquid in sequence, charges on the surface of the silicon wafer are neutralized, and adhesion of the large particles is avoided; and slow lifting and drying are carried out in the static electricity eliminating device, so that ion charges in the environment and static electricity on the surface of the silicon wafer are neutralized, the cleanliness of the surface of the silicon wafer is further ensured, and large particles are not adsorbed any more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field, and relates to a method for reducing large particles on the surface of a silicon wafer before single-sided grinding, and in particular to a method for reducing large particles on the surface of a silicon wafer before single-sided grinding, a grinding method and a silicon wafer. Background Art

[0002] With the booming development of industries such as integrated circuits, artificial intelligence and big data, product applications are becoming more and more extensive; driven by the ever-expanding global demand, major semiconductor companies are constantly expanding new plants and increasing production capacity to meet market demand; at the same time, the performance of continuously iterated application products is constantly upgrading, which has put forward higher requirements for chip integration, energy consumption and computing speed. These higher demands on the application side continue to give birth to chip products with smaller line widths, lower energy consumption and faster computing speeds. In the process of continuously launching iterative upgraded products, they often face greater losses in process yield. In particular, the production and processing of 300mm large-size silicon wafers for integrated circuits has strict requirements for high flatness and high cleanliness, which run through the entire process of 300mm large-size silicon wafer processing.

[0003] The main links in the manufacturing process of 300mm large-size silicon wafers for integrated circuits include crystal growth, crystal rod forming, silicon wafer forming, double-sided polishing and cleaning. Among them, the process capability of silicon wafer forming directly determines the flatness level of silicon wafers. It is a key process step that lays the foundation for silicon wafer quality and connects the previous and the next. The so-called silicon wafer forming includes processes such as crystal rod cutting, silicon wafer chamfering and silicon wafer grinding. After these processes are completed, the general morphology of the silicon wafer has been basically determined. Silicon wafer chamfering mainly determines the edge morphology of the silicon wafer, crystal rod cutting mainly determines the overall morphology of the silicon wafer, and silicon wafer grinding mainly affects the local morphological characteristics of the silicon wafer.

[0004] Silicon wafer grinding is further divided into double-sided grinding and single-sided grinding. The mainstream process is double-sided grinding plus single-sided grinding to complete silicon wafer grinding. The process route of double-sided grinding plus single-sided grinding of silicon wafers will inevitably lead to the situation where the results of the previous process affect the subsequent process. The grinding sand and silicon powder remaining on the surface of the double-sided grinding of silicon wafers will seriously affect the accuracy of single-sided grinding of silicon wafers. This is because single-sided grinding of silicon wafers is that one side of the silicon wafer is vacuum adsorbed on a carrier disk with ultra-high flatness and the other side is ground with a high-precision grinding wheel. If there are large particles on the surface of the vacuum adsorbed silicon wafer, it will cause convexity or concave morphology of the local morphology of the silicon wafer. At the same time, the presence of large particles will also cause hard damage such as small pits on the surface of the vacuum adsorbed silicon wafer.

[0005] CN117491321A discloses a method for detecting heavily-boron-doped defects, which belongs to the field of silicon wafer processing technology, and includes the following operating steps: Step 1: After the heavily-boron-doped single crystal silicon rod is wire-cut, one silicon wafer is drawn out of every 50 wafers to form a leading wafer. Step 2: The leading wafer is double-sided ground for primary chamfering and single-sided ground for secondary chamfering. Step 3: Alkaline etching is performed after secondary chamfering. Step 4: The leading wafer is placed in a cleaning tank with a mixture of HCl and H2O2 for cleaning. Step 5: After cleaning and drying, the surface defects of the silicon wafer are checked with a fluorescent lamp. Step 6: The qualified leading wafer is double-sided polished. Step 7: After polishing, it is cleaned with a tank cleaning machine. Step 8: Single-sided polishing is performed. Step 9: The silicon wafer after single-sided polishing is returned to alkaline etching again. Step 10: After cleaning and drying, the surface defects of the silicon wafer are checked with a fluorescent lamp.

[0006] CN115579281A discloses a method for improving the focusing anomaly of a 12-inch wafer after photolithography, which belongs to the field of semiconductor processing technology, and includes the following operating steps: Step 1: Processing and polishing silicon wafers, first chamfering, then double-sided grinding, then single-sided grinding, and then secondary chamfering, followed by laser engraving, followed by alkaline corrosion, and the next step is double-sided polishing and cleaning. After cleaning, edge polishing is performed, and then single-sided polishing is performed, and finally cleaning is performed again. Step 2: Select qualified polished silicon wafers, and rework unqualified polished silicon wafers. Step 3: After applying photoresist, perform automatic optical inspection to check whether there will be focusing anomalies during the inspection process. Step 4: Rework the polished silicon wafers that have focusing anomalies during the automatic optical inspection.

[0007] The currently disclosed methods for reducing large particles on the surface of silicon wafers before single-sided grinding have certain defects, such as incomplete cleaning of large particles on the surface of silicon wafers before single-sided grinding, and adsorption of large particles during subsequent single-sided grinding, which results in a low yield rate of silicon wafers after grinding. Therefore, it is very important to develop a new method for reducing large particles on the surface of silicon wafers before single-sided grinding, a grinding method, and a silicon wafer after grinding. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention aims to provide a method for reducing large particles on the surface of a silicon wafer before single-sided grinding, a grinding method and a silicon wafer. In the method provided by the present invention, ultrasonic cleaning with a cleaning liquid is used to achieve preliminary cleaning of large particles adsorbed on the surface of the silicon wafer; then, cleaning with a cleaning liquid and cleaning with a moisturizing liquid are performed in sequence to further clean the large particles contaminated on the surface of the silicon wafer, and neutralize the charge on the surface of the silicon wafer to avoid the adhesion of large particles; then, slow pulling and drying in an electrostatic eliminator is performed to neutralize the ionic charge in the environment and the static electricity on the surface of the silicon wafer, further ensuring the cleanliness of the surface of the silicon wafer and preventing the adsorption of large particles; therefore, after reducing large particles on the surface of the silicon wafer before single-sided grinding by the method, single-sided grinding is performed, and the yield rate of the ground silicon wafer is high.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for reducing large particles on a silicon wafer surface before single-side grinding, the method comprising:

[0011] The silicon wafer is cleaned before single-side grinding; the cleaning includes ultrasonic cleaning with a cleaning liquid, cleaning with a cleaning liquid, cleaning with a moisturizing liquid and slow pulling and drying in sequence, and the slow pulling and drying is performed in an electrostatic elimination device.

[0012] In the method provided by the present invention, the large particles adsorbed on the surface of the silicon wafer are initially cleaned by ultrasonic cleaning with a cleaning liquid; the large particles contaminated on the surface of the silicon wafer are further cleaned by cleaning with a cleaning liquid and cleaning with a moisturizing liquid in sequence, and the charge on the surface of the silicon wafer is neutralized to avoid the adhesion of large particles; and the ionic charge in the environment and the static electricity on the surface of the silicon wafer are neutralized by slow pulling and drying in an electrostatic eliminator, thereby further ensuring the cleanliness of the surface of the silicon wafer and preventing the adsorption of large particles; therefore, after reducing the large particles on the surface of the silicon wafer before single-side grinding by the method, single-side grinding is performed, and the yield rate of the ground silicon wafer is high.

[0013] Preferably, the ultrasonic cleaning with cleaning liquid comprises: placing the silicon wafer in the cleaning liquid and performing ultrasonic treatment.

[0014] Preferably, the temperature of the ultrasonic cleaning with the cleaning liquid is 40 to 70° C., and the time is 3 to 10 minutes.

[0015] The temperature of ultrasonic cleaning with the cleaning liquid in the present invention is 40-70°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] The time for ultrasonic cleaning with the cleaning liquid in the present invention is 3 to 10 minutes, for example, it can be 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, 6.5 minutes, 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes or 10 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, water flushing cleaning is also included between the cleaning liquid ultrasonic cleaning and the cleaning liquid cleaning.

[0018] The water used in the water flushing and cleaning of the present invention includes ultrapure water.

[0019] Preferably, the cleaning with cleaning liquid comprises: placing the silicon wafer in the cleaning liquid.

[0020] Preferably, the cleaning temperature of the cleaning solution is 40-70° C., and the cleaning time is 3-10 min.

[0021] The cleaning temperature of the cleaning liquid in the present invention is 40-70°C, for example, it can be 40°C, 42°C, 45°C, 47°C, 50°C, 52°C, 55°C, 57°C, 60°C, 62°C, 65°C, 67°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] The cleaning time of the cleaning solution in the present invention is 3 to 10 minutes, for example, it can be 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the mass concentration of the cleaning agent in the cleaning liquid in the cleaning liquid ultrasonic cleaning and the cleaning liquid cleaning is independently 2 to 6wt%, for example, it can be 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt% or 6wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent as percentage, the mass fraction of potassium hydroxide in the cleaning agent is 20-30wt%, the mass fraction of pyrophosphoric acid is 10-15wt%, the mass fraction of disodium silicate is 5-10wt%, the mass fraction of the surfactant is 5-10wt%, and the balance is water.

[0025] In the present invention, the mass fraction of potassium hydroxide in the cleaning agent is 20-30wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt% or 30wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] In the present invention, the mass fraction of pyrophosphoric acid in the cleaning agent is 10-15wt%, for example, it can be 10wt%, 10.5wt%, 11wt%, 11.5wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt%, 14.5wt% or 15wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In the present invention, based on the mass of the cleaning agent as percentage, the mass fraction of disodium silicate is 5 to 10wt%, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In the present invention, the mass fraction of the surfactant is 5-10wt% based on the mass of the cleaning agent, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] The surfactant described in the present invention is any surfactant that has been disclosed in the prior art and can be used in cleaning agents.

[0030] The water in the cleaning agent of the present invention is preferably ultrapure water.

[0031] Preferably, the moisturizing liquid cleaning comprises: placing the silicon wafer in the moisturizing liquid.

[0032] Preferably, the temperature of the moisturizing liquid cleaning is 20-26° C., and the time is 3-10 minutes.

[0033] The temperature for washing with the moisturizing solution in the present invention is 20-26°C, for example, it can be 20°C, 20.5°C, 21°C, 21.5°C, 22°C, 22.5°C, 23°C, 23.5°C, 24°C, 24.5°C, 25°C, 25.5°C or 26°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] The cleaning time of the moisturizing liquid in the present invention is 3 to 10 minutes, for example, it can be 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, 6.5 minutes, 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes or 10 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the moisturizing solution is obtained by diluting the moisturizing agent 60 to 100 times, for example, 60 times, 65 times, 70 times, 75 times, 80 times, 85 times, 90 times, 95 times or 100 times, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the moisturizing agent consists of rosin, aliphatic polyol, glycol solvent and water.

[0037] Preferably, based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 40-50wt%, for example, it can be 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% or 50wt%.

[0038] The mass fractions of the aliphatic polyol, glycol solvent and water in the moisturizing agent of the present invention are not limited.

[0039] The glycol solvent described in the present invention includes DRYNON C produced by Nichika Seiko Co., Ltd.

[0040] The water in the moisturizing agent of the present invention is preferably ultrapure water.

[0041] Preferably, water overflow cleaning is further included between the moisturizing liquid cleaning and the slow pull drying.

[0042] Preferably, the pulling speed of the slow pulling drying is 0.8 to 3 mm / s, for example, it can be 0.8 mm / s, 1 mm / s, 1.2 mm / s, 1.4 mm / s, 1.6 mm / s, 1.8 mm / s, 2 mm / s, 2.2 mm / s, 2.4 mm / s, 2.6 mm / s, 2.8 mm / s or 3 mm / s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the temperature of the slow pulling drying is 23-60°C, for example, 23°C, 26°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] As a preferred technical solution of the method of the present invention, the method comprises:

[0045] At 40-70°C, the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 2-6wt% for ultrasonic treatment for 3-10 minutes, and then washed with water; then, at 40-70°C, the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 2-6wt% for 3-10 minutes; then, at 20-26°C, the silicon wafer is placed in a moisturizing solution obtained by diluting the moisturizing agent 60-100 times for 3-10 minutes, and then washed with water overflow; then, in an electrostatic eliminator, at 23-60°C, the silicon wafer is pulled and dried at a pulling speed of 0.8-3mm / s, and then single-sided grinding is performed.

[0046] In a second aspect, the present invention provides a method for grinding a silicon wafer, the method comprising: grinding the silicon wafer on both sides, reducing large particles on the surface of the silicon wafer, and then grinding the silicon wafer on one side.

[0047] Preferably, reducing large particles on the surface of the silicon wafer is carried out by the method described in the first aspect.

[0048] Preferably, the silicon wafer is a silicon wafer with a silicon wafer diameter of not less than 300 mm, including a 12-inch (300 mm) silicon wafer and an 18-inch (450 mm) silicon wafer.

[0049] Preferably, the double-side grinding and the reduction of large particles on the surface of the silicon wafer further include brushing, chamfering and water washing in sequence.

[0050] In a third aspect, the present invention provides a ground silicon wafer, which is obtained by the grinding method described in the second aspect, and the yield rate of the ground silicon wafer is not less than 99%, for example, it can be 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8% or 99.9% or 99%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] In the method provided by the present invention, the large particles adsorbed on the surface of the silicon wafer are initially cleaned by ultrasonic cleaning with a cleaning liquid; the large particles contaminated on the surface of the silicon wafer are further cleaned by cleaning with a cleaning liquid and cleaning with a moisturizing liquid in sequence, and the charge on the surface of the silicon wafer is neutralized to avoid the adhesion of large particles; and the ionic charge in the environment and the static electricity on the surface of the silicon wafer are neutralized by slow pulling and drying in an electrostatic eliminator, thereby further ensuring the cleanliness of the surface of the silicon wafer and preventing the adsorption of large particles; therefore, after reducing the large particles on the surface of the silicon wafer before single-side grinding by the method, single-side grinding is performed, and the yield rate of the ground silicon wafer is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The present invention is a flow chart of a method for grinding a silicon wafer having a diameter of 300 mm. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0055] Example 1

[0056] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, the method comprising:

[0057] At 55°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 4wt% of the cleaning agent for 6 minutes of ultrasonic treatment, and then rinsed with water; then placed in a cleaning solution with a mass concentration of 4wt% of the cleaning agent at 55°C for 6 minutes; then placed in a moisturizing solution obtained by diluting the moisturizing agent 80 times at 23°C for 6 minutes, and then rinsed with water; then pulled and dried at a pulling speed of 2mm / s at 40°C in an electrostatic eliminator, and then single-sided grinding was performed;

[0058] The cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent, the mass fraction of potassium hydroxide in the cleaning agent is 25wt%, the mass fraction of pyrophosphoric acid is 12wt%, the mass fraction of disodium silicate is 8wt%, the mass fraction of the surfactant is 8wt%, and the balance is water;

[0059] The moisturizing agent consists of rosin, aliphatic polyol, glycol solvent and water, wherein the glycol solvent is DRYNON C produced by Nichika Seiko Co., Ltd.; based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 45wt%, the mass fraction of aliphatic polyol is 5wt%, the mass fraction of glycol solvent is 10wt%, and the balance is water.

[0060] Example 2

[0061] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, the method comprising:

[0062] At 45°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 5wt% of the cleaning agent for 4 minutes of ultrasonic treatment, and then rinsed with water; then at 70°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 2wt% of the cleaning agent for 5 minutes; then at 25°C, the silicon wafer was placed in a moisturizing solution obtained by diluting the moisturizing agent 60 times for 10 minutes, and then rinsed with water; then in an electrostatic eliminator, at 50°C, the silicon wafer was pulled and dried at a pulling speed of 1.4mm / s, and then single-sided grinding was performed;

[0063] The cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent, the mass fraction of potassium hydroxide in the cleaning agent is 20wt%, the mass fraction of pyrophosphoric acid is 15wt%, the mass fraction of disodium silicate is 5wt%, the mass fraction of the surfactant is 10wt%, and the balance is water;

[0064] The moisturizing agent is composed of rosin, aliphatic polyol, glycol solvent and water, wherein the glycol solvent is DRYNON C produced by Nichika Seiko Co., Ltd.; based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 40wt%, the mass fraction of aliphatic polyol is 15wt%, the mass fraction of glycol solvent is 5wt%, and the balance is water.

[0065] Example 3

[0066] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, the method comprising:

[0067] At 40°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 3wt% of the cleaning agent for 10 minutes of ultrasonic treatment, and then rinsed with water; then at 65°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 3wt% of the cleaning agent for 10 minutes; then at 20°C, the silicon wafer was placed in a moisturizing solution obtained by diluting the moisturizing agent 90 times for 4 minutes, and then rinsed with water; then in an electrostatic eliminator, at 23°C, the silicon wafer was pulled and dried at a pulling speed of 0.8mm / s, and then single-sided grinding was performed;

[0068] The cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent, the mass fraction of potassium hydroxide in the cleaning agent is 30wt%, the mass fraction of pyrophosphoric acid is 10wt%, the mass fraction of disodium silicate is 10wt%, the mass fraction of the surfactant is 5wt%, and the balance is water;

[0069] The moisturizing agent consists of rosin, aliphatic polyol, glycol solvent and water, wherein the glycol solvent is DRYNON C produced by Nichika Seiko Co., Ltd.; based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 50wt%, the mass fraction of aliphatic polyol is 8wt%, the mass fraction of glycol solvent is 12wt%, and the balance is water.

[0070] Example 4

[0071] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, the method comprising:

[0072] At 70°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 2wt% of the cleaning agent for 8 minutes of ultrasonic treatment, and then rinsed with water; then at 40°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 5wt% of the cleaning agent for 8 minutes; then at 26°C, the silicon wafer was placed in a moisturizing solution obtained by diluting the moisturizing agent 100 times for 8 minutes, and then rinsed with water; then in an electrostatic eliminator, it was pulled and dried at a pulling speed of 3mm / s at 60°C, and then single-sided grinding was performed;

[0073] The cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent, the mass fraction of potassium hydroxide in the cleaning agent is 25wt%, the mass fraction of pyrophosphoric acid is 12wt%, the mass fraction of disodium silicate is 8wt%, the mass fraction of the surfactant is 8wt%, and the balance is water;

[0074] The moisturizing agent consists of rosin, aliphatic polyol, glycol solvent and water, wherein the glycol solvent is DRYNON C produced by Nichika Seiko Co., Ltd.; based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 45wt%, the mass fraction of aliphatic polyol is 5wt%, the mass fraction of glycol solvent is 10wt%, and the balance is water.

[0075] Example 5

[0076] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding, the method comprising:

[0077] At 65°C, the silicon wafer was placed in a cleaning solution with a mass concentration of 6wt% of the cleaning agent for 3 minutes of ultrasonic treatment, and then rinsed with water; then placed in a cleaning solution with a mass concentration of 6wt% of the cleaning agent at 45°C for 3 minutes; then placed in a moisturizing solution obtained by diluting the moisturizing agent 70 times at 22°C for 3 minutes, and then rinsed with water; then pulled and dried at a pulling speed of 2.5mm / s at 30°C in an electrostatic eliminator, and then single-sided grinding was performed;

[0078] The cleaning agent comprises potassium hydroxide, pyrophosphoric acid, disodium silicate, a surfactant and water; based on the mass of the cleaning agent, the mass fraction of potassium hydroxide in the cleaning agent is 25wt%, the mass fraction of pyrophosphoric acid is 12wt%, the mass fraction of disodium silicate is 8wt%, the mass fraction of the surfactant is 8wt%, and the balance is water;

[0079] The moisturizing agent consists of rosin, aliphatic polyol, glycol solvent and water, wherein the glycol solvent is DRYNON C produced by Nichika Seiko Co., Ltd.; based on the mass of the moisturizing agent as 100%, the mass fraction of rosin in the moisturizing agent is 45wt%, the mass fraction of aliphatic polyol is 5wt%, the mass fraction of glycol solvent is 10wt%, and the balance is water.

[0080] Example 6

[0081] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. Except that the silicon wafer is placed in a cleaning agent for ultrasonic treatment at 30° C., the rest is the same as that of Embodiment 1.

[0082] Example 7

[0083] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. Except that the silicon wafer is placed in a cleaning agent for ultrasonic treatment at 90° C., the rest is the same as that of Embodiment 1.

[0084] Example 8

[0085] This embodiment provides a method for reducing large particles on the surface of silicon wafers before single-side grinding. Except that the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 1 wt % for ultrasonic treatment, the rest is the same as that of embodiment 1.

[0086] Example 9

[0087] This embodiment provides a method for reducing large particles on the surface of silicon wafers before single-side grinding. Except that the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 8 wt % for ultrasonic treatment, the rest is the same as that of embodiment 1.

[0088] Example 10

[0089] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. The method is the same as that of Embodiment 1 except that the silicon wafer is placed in a moisturizing solution diluted with a moisturizing agent at 15°C.

[0090] Embodiment 11

[0091] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. The method is the same as that of Embodiment 1 except that the silicon wafer is placed in a moisturizing solution diluted with a moisturizing agent at 35°C.

[0092] Example 12

[0093] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. The method is the same as that of Embodiment 1 except that the silicon wafer is placed in a moisturizing solution obtained by diluting the moisturizing agent 40 times.

[0094] Embodiment 13

[0095] This embodiment provides a method for reducing large particles on the surface of a silicon wafer before single-side grinding. The method is the same as that of Embodiment 1 except that the silicon wafer is placed in a moisturizing solution obtained by diluting the moisturizing agent 120 times.

[0096] Embodiment 14

[0097] This embodiment provides a method for reducing large particles on the surface of silicon wafers before single-sided grinding. Except for the pulling and drying at a pulling speed of 0.6 mm / s, the rest is the same as that of Embodiment 1.

[0098] Embodiment 15

[0099] This embodiment provides a method for reducing large particles on the surface of silicon wafers before single-sided grinding. Except for the pulling and drying at a pulling speed of 3.5 mm / s, the rest is the same as that of Embodiment 1.

[0100] Comparative Example 1

[0101] This comparative example provides a method for reducing large particles on the surface of silicon wafers before single-sided grinding, which is the same as Example 1 except that the ultrasonic treatment of the silicon wafer in a cleaning solution with a cleaning agent concentration of 4 wt % at 55° C. for 6 min is omitted.

[0102] Comparative Example 2

[0103] This comparative example provides a method for reducing large particles on the surface of silicon wafers before single-sided grinding, except that the steps of placing the silicon wafer in a cleaning solution with a cleaning agent concentration of 4wt% at 55°C for 6 minutes and placing the silicon wafer in a moisturizing solution obtained by diluting the moisturizing agent 80 times at 23°C for 6 minutes are omitted, and the rest are the same as Example 1.

[0104] Comparative Example 3

[0105] This comparative example provides a method for reducing large particles on the surface of silicon wafers before single-sided grinding, except that the pulling and drying at a pulling speed of 2 mm / s at 40°C in the static eliminator is omitted, and the rest is the same as Example 1.

[0106] like Figure 1 As shown, a silicon wafer with a diameter of 300 mm before grinding is double-sided ground, and then brushed, chamfered and rinsed with water in sequence, and then the method provided in the above embodiment and comparative example is used to reduce large particles on the surface of the silicon wafer, and then single-sided grinding is performed to obtain a ground silicon wafer; the yield rate of the obtained ground silicon wafer is tested, and the yield rate of the ground silicon wafer is shown in Table 1.

[0107] Table 1

[0108]

[0109]

[0110] From Table 1, we can get:

[0111] (1) After the silicon wafer before grinding is treated by the method for reducing large particles on the surface of the silicon wafer before single-side grinding provided in Examples 1 to 5, the silicon wafer after grinding finally obtained has a higher yield;

[0112] (2) By comparing Example 1 with Examples 6 and 7, it can be seen that the temperature of the ultrasonic cleaning of the cleaning liquid in the present invention will affect the yield rate of the finally obtained silicon wafer after grinding; when the temperature of the ultrasonic cleaning of the cleaning liquid is low, the yield rate of the silicon wafer after grinding will be low, because the low temperature causes the chemical reaction rate to be low, which in turn causes the cleaning liquid to be insufficiently active and reduces the cleaning efficiency; when the temperature of the ultrasonic cleaning of the cleaning liquid is high, the yield rate of the silicon wafer after grinding will be low, because the high temperature causes the active ingredients in the cleaning liquid to decompose due to high temperature, lose their original chemical properties, and thus reduce the cleaning efficiency;

[0113] (3) By comparing Example 1 with Examples 8 and 9, it can be seen that the mass concentration of the cleaning agent in the cleaning solution in the ultrasonic cleaning of the cleaning solution described in the present invention will affect the yield rate of the silicon wafers finally obtained after grinding; when the mass concentration of the cleaning agent is low, the yield rate of the silicon wafers after grinding will be low, because the mass concentration of the cleaning agent is low, resulting in less effective ingredients in the cleaning solution, thereby weakening the cleaning effect; when the mass concentration of the cleaning agent is high, the yield rate of the silicon wafers after grinding will be low, because the mass concentration of the cleaning agent is high, resulting in too high pH of the cleaning solution, thereby causing an over-corrosion effect on the silicon wafer, forming corrosion pits on the surface of the silicon wafer, thereby reducing the yield rate;

[0114] (4) By comparing Example 1 with Examples 10 and 11, it can be seen that the temperature of the moisturizing solution cleaning in the present invention will affect the yield rate of the finally obtained silicon wafer after grinding; when the temperature of the moisturizing solution cleaning is low, the yield rate of the silicon wafer after grinding will be lowered, because the low temperature causes the physicochemical activity of the moisturizing solution to decrease, thereby affecting the cleaning efficiency; when the temperature of the moisturizing solution cleaning is high, the yield rate of the silicon wafer after grinding will be lowered, because the high temperature causes the active ingredients in the moisturizing solution to lose their original chemical properties due to high-temperature decomposition, thereby reducing the cleaning efficiency;

[0115] (5) By comparing Example 1 with Examples 12 and 13, it can be seen that the concentration of the moisturizing liquid in the moisturizing liquid cleaning of the present invention will affect the yield rate of the finally obtained silicon wafer after grinding; when the concentration of the moisturizing liquid is low, the yield rate of the silicon wafer after grinding will be low, because the concentration of the moisturizing liquid is low, resulting in less effective ingredients in the moisturizing liquid, thereby weakening the cleaning effect; when the concentration of the moisturizing liquid is high, the yield rate of the silicon wafer after grinding will be low, because the concentration of the moisturizing liquid is high, which will make it difficult to clean the residual moisturizing liquid on the silicon wafer in the subsequent process of ultrapure water overflow cleaning, thereby affecting the slow pull-drying effect of the final silicon wafer;

[0116] (6) By comparing Example 1 with Examples 14 and 15, it can be seen that the pulling speed of the slow pulling and drying in the present invention will affect the yield rate of the finally obtained silicon wafer after grinding; when the slow pulling speed is too slow, the efficiency of the method for reducing large particles on the surface of the silicon wafer before single-sided grinding will be too low, thereby resulting in a decrease in production capacity; when the slow pulling speed is too fast, the yield rate of the silicon wafer after grinding will be lowered. This is because the slow pulling speed is too fast, which will cause the surface of the silicon wafer to be not dry and have water droplets. The presence of water droplets will easily absorb large particles in the environment;

[0117] (7) By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that in the method provided by the present invention, the large particles adsorbed on the surface of the silicon wafer are initially cleaned by ultrasonic cleaning with a cleaning liquid; then, by successively cleaning with a cleaning liquid and cleaning with a moisturizing liquid, the large particles contaminated on the surface of the silicon wafer are further cleaned, and the charge on the surface of the silicon wafer is neutralized to avoid the adhesion of large particles; then, by slow pulling and drying in an electrostatic eliminator, the ionic charge in the environment and the static electricity on the surface of the silicon wafer are neutralized, further ensuring the cleanliness of the surface of the silicon wafer and preventing the adsorption of large particles; therefore, after reducing the large particles on the surface of the silicon wafer before single-sided grinding by the method, single-sided grinding is performed, and the yield rate of the ground silicon wafer is higher.

[0118] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for reducing large particles on the surface of a silicon wafer before single-side grinding, characterized in that: The method comprises: The silicon wafer is cleaned before single-side grinding; the cleaning includes ultrasonic cleaning with a cleaning liquid, cleaning with a cleaning liquid, cleaning with a moisturizing liquid and slow pulling and drying in sequence, and the slow pulling and drying is performed in an electrostatic elimination device.

2. The method according to claim 1, characterized in that The cleaning solution ultrasonic cleaning comprises: placing the silicon wafer in the cleaning solution for ultrasonic treatment; Preferably, the temperature of the cleaning solution ultrasonic cleaning is 40-70°C and the time is 3-10 minutes; Preferably, water flushing cleaning is also included between the cleaning liquid ultrasonic cleaning and the cleaning liquid cleaning.

3. The method according to claim 1 or 2, characterized in that: The cleaning solution cleaning comprises: placing the silicon wafer in the cleaning solution; Preferably, the cleaning temperature of the cleaning solution is 40-70° C., and the cleaning time is 3-10 min.

4. The method according to any one of claims 1 to 3, characterized in that: The mass concentration of the cleaning agent in the cleaning liquid ultrasonic cleaning and the cleaning liquid cleaning is independently 2-6wt%.

5. The method according to any one of claims 1 to 4, characterized in that: The moisturizing liquid cleaning comprises: placing the silicon wafer in the moisturizing liquid; Preferably, the temperature of the moisturizing solution cleaning is 20-26°C and the time is 3-10 minutes; Preferably, the moisturizing solution is obtained by diluting the moisturizing agent 60 to 100 times; Preferably, the moisturizing agent is composed of rosin, aliphatic polyol, glycol solvent and water; Preferably, water overflow cleaning is further included between the moisturizing liquid cleaning and the slow pull drying.

6. The method according to any one of claims 1 to 5, characterized in that: The pulling speed of the slow pulling drying is 0.8 to 3 mm / s; Preferably, the temperature of the slow pulling drying is 23-60°C.

7. The method according to any one of claims 1 to 6, characterized in that: The method comprises: At 40-70°C, the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 2-6wt% for ultrasonic treatment for 3-10 minutes, and then washed with water; then, at 40-70°C, the silicon wafer is placed in a cleaning solution with a cleaning agent concentration of 2-6wt% for 3-10 minutes; then, at 20-26°C, the silicon wafer is placed in a moisturizing solution obtained by diluting the moisturizing agent 60-100 times for 3-10 minutes, and then washed with water overflow; then, in an electrostatic eliminator, at 23-60°C, the silicon wafer is pulled and dried at a pulling speed of 0.8-3mm / s, and then single-sided grinding is performed.

8. A method for grinding a silicon wafer, characterized in that: The grinding method comprises: grinding the silicon wafer on both sides to reduce large particles on the surface of the silicon wafer, and then grinding the silicon wafer on one side; Preferably, reducing large particles on the surface of the silicon wafer is carried out by the method described in any one of claims 1 to 7.

9. The grinding method according to claim 8, characterized in that: The silicon wafer is a silicon wafer with a diameter of not less than 300 mm; Preferably, the double-side grinding and the reduction of large particles on the surface of the silicon wafer further include brushing, chamfering and water washing in sequence.

10. A ground silicon wafer, characterized in that: The ground silicon wafer is obtained by the grinding method according to claim 8 or 9, and the yield rate of the ground silicon wafer is not less than 99%.

Citation Information

Patent Citations

  • Silicon wafer cleaning agent and silicon wafer cleaning method

    CN108300583A

  • Cleaning agent and cleaning method used for polished glass

    CN109609290A

  • Cleaning method of ultra-large-size single crystal silicon wafer

    CN110665893A

  • Cleaning process for improving surface cleanliness of edge-polished large-diameter silicon wafer

    CN111211042A

  • Physical cleaning method of silicon wafer

    CN111330903A