High-strength shaving board and preparation method thereof
Through the combination technology of corn starch modified shavings and urea formaldehyde resin adhesive, the problem of water absorption and expansion of traditional particleboard in high humidity environments is solved, the water resistance and mechanical properties of particleboard are improved, and a more stable bonding layer is formed, which is enhanced. Overall performance.
Patent Information
- Application Number
- CN202411353172.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional particle boards are prone to absorb water and expand and deform in environments with high humidity, resulting in reduced mechanical properties and unstable structural factors, which increase safety hazards during use.
The combination method of corn starch modified shavings and urea-formaldehyde resin adhesive is used to modify shavings through sodium hydroxide regulation solution and ultrasonic dispersion technology, and combine silane coupling agent and oxidized corn starch to form a tighter network structure to improve water resistance. and mechanical properties.
It significantly improves the water resistance and mechanical properties of particleboard, forms a denser bonding layer, prevents moisture penetration, and enhances the overall stability and strength of the board.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of particle boards, and in particular to a high-strength particle board and a preparation method thereof. Background Art
[0002] Traditional particleboard, as an important member of wood composite materials, has a simple production process and high cost-effectiveness, and occupies a pivotal position in many industries. By mixing wood shavings with an appropriate amount of adhesive and pressing them under high temperature and high pressure, this material not only retains the natural texture of wood, but also has good processing performance and plasticity, and is easy to cut, drill and assemble, providing rich design space and flexible application options for furniture manufacturing, building decoration and packaging industries.
[0003] However, despite the many advantages of traditional particleboard, its mechanical properties and water resistance cannot be taken into account, which is a problem that cannot be ignored. In environments with high humidity such as bathrooms, kitchens, and basements, moisture can easily penetrate into the interior of the particleboard, causing the board to absorb water and swell, deform, and even cause surface cracking and falling off. This physical change not only destroys the aesthetics of the particleboard, but more importantly, it seriously affects the mechanical properties and structural stability of the board. With the continuous erosion of moisture, the internal structure of the particleboard gradually disintegrates, the strength is significantly reduced, and it can no longer withstand the original load, thereby increasing the safety hazards during use.
[0004] In this regard, the present invention proposes an innovative high-strength particleboard and a unique preparation method thereof, aiming to improve the mechanical properties and water resistance of the particleboard and broaden its application fields. Summary of the invention
[0005] The present invention provides a high-strength particleboard and a preparation method thereof. By preparing corn starch-modified particles and compounding them with a urea-formaldehyde resin adhesive, the mechanical properties of the particleboard can be ensured while also improving the water resistance of the board.
[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a high-strength particleboard, comprising corn starch modified particles and an adhesive in a weight ratio of (10-12): (0.1-0.2); wherein the preparation method of the corn starch modified particles comprises: crushing the particles, soaking them in a sodium hydroxide solution, washing and drying them, adding them to anhydrous ethanol for ultrasonic dispersion, and then adding a silane coupling agent and oxidized corn starch and stirring and mixing them to obtain the particleboard.
[0007] As a further technical solution, the moisture content of the wood chips is 4%-5%, the mass concentration of the sodium hydroxide solution is 6%-8%, and the immersion time is 10-15 minutes.
[0008] As a further technical solution, the ultrasonic dispersion time is 20-30 minutes.
[0009] As a further technical solution, the stirring and mixing speed is 200-240r / min, the stirring and mixing time is 1-1.2h, and the mixture is allowed to stand for 20-30min after stirring.
[0010] As a further technical solution, the weight ratio of the wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20: (30-40): (0.2-0.4): (0.5-1).
[0011] As a further technical solution, the preparation method of the oxidized corn starch includes: adding deionized water to corn starch to form a starch mixture with a mass ratio of 30%-32%, adding sodium hydroxide to condition the solution to have a pH of 12, stirring at a temperature of 40-46°C and adding potassium permanganate consistent with the starch content, keeping the temperature constant, adding sulfuric acid consistent with the starch content, washing and filtering when the solution turns pure white, and drying at a temperature of 50-60°C to obtain the product.
[0012] As a further technical solution, the adhesive is a urea-formaldehyde resin adhesive.
[0013] In a second aspect, the present invention proposes a method for preparing a high-strength particleboard, the steps comprising: stirring and mixing the modified wood particles and an adhesive, paving them in a mold, pre-pressing the paved board, then hot pressing and cooling, and trimming and sanding the hot-pressed board.
[0014] As a further technical solution, the pre-pressing temperature is 190-200°C, the pre-pressing time is 25-35min, and the pre-pressing pressure is 2-3MPa.
[0015] As a further technical solution, the hot pressing temperature is 110-120°C, the hot pressing time is 8-10 minutes, and the hot pressing pressure is 2-3MPa.
[0016] The working principle and beneficial effects of the present invention are: The present invention can induce the oxidation reaction of starch molecules by adding sodium hydroxide to adjust the solution to an alkaline environment (pH=12), and adding potassium permanganate at a suitable temperature (43°C). The oxidation reaction will introduce hydrophilic functional groups such as carboxyl and aldehyde groups, but it may also increase the cross-linking degree of starch molecules to form a tighter network structure. Subsequently, sulfuric acid is added for neutralization reaction. When the solution turns pure white, it indicates that the oxidation reaction is basically completed. The molecular structure of the oxidized corn starch obtained after washing, filtration and drying has changed, and has better water resistance and stability. When preparing corn starch modified wood chips, the wood chips are first impregnated with a sodium hydroxide solution to improve their surface roughness and wettability, which is conducive to the attachment of subsequent adhesives. Subsequently, by ultrasonic dispersion in anhydrous ethanol, the fiber structure of the wood chips can be further opened to increase their specific surface area. After adding a silane coupling agent, one end of the silane coupling agent can react with functional groups such as hydroxyl groups on the surface of the wood chips, and the other end can combine with functional groups in the oxidized corn starch, thereby forming a strong chemical bond between the wood chips and the starch. The formation of this chemical bond not only enhances the bonding between the wood chips, but also improves the water resistance of the board. Because the silane coupling agent itself has excellent waterproof properties, it can effectively prevent moisture from penetrating into the board. Urea-formaldehyde resin, as a commonly used wood adhesive, has good bonding properties, but its water resistance is relatively poor. However, when used in combination with corn starch modified wood chips, the water resistance of particleboard can be significantly improved. First, the oxidized corn starch and silane coupling agent in the corn starch modified wood chips have provided strong bonding and certain water resistance between the wood chips. When these modified wood chips are mixed with urea-formaldehyde resin, urea-formaldehyde resin can further fill the gaps between the wood chips to form a denser board structure. This structural density helps to prevent water penetration. Secondly, urea-formaldehyde resin will form a three-dimensional network structure during the curing process, which will firmly bond the wood chips together. The oxidized corn starch and silane coupling agent in the corn starch modified wood chips can serve as reinforcement points for this network structure, improving the stability and strength of the entire network structure. This enhanced network structure not only improves the mechanical properties of the board, but also enhances its water resistance. Finally, the oxidized corn starch and silane coupling agent in the corn starch modified wood chips are combined with the urea-formaldehyde resin to further enhance their compatibility and adhesion. This enhanced compatibility and adhesion help to form a more uniform and dense bonding layer inside the board, thereby improving the overall water resistance of the board. DETAILED DESCRIPTION The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In the present invention, the urea-formaldehyde resin adhesive is an E1-level environmentally friendly urea-formaldehyde resin adhesive purchased from Jinan Qianlai Environmental Protection Technology Co., Ltd.; the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane; the pulverized wood chips have a length of 10-12 mm, a width of 5-6 mm, and a thickness of 0.5-0.6 mm.
[0018] Example 1 The present embodiment provides a high-strength particle board, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 31%, add sodium hydroxide to adjust the solution pH to 12, stir at 43°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 55°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: wood chips with a moisture content of 4.5% were crushed and immersed in a 7% sodium hydroxide solution for 12 minutes, then washed and dried, added to anhydrous ethanol and ultrasonically dispersed for 25 minutes, and then silane coupling agent and oxidized corn starch were added and stirred and mixed. The stirring speed was 220 r / min, the stirring time was 1.1 h, and the mixture was allowed to stand for 25 minutes after stirring. The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20:35:0.3:0.7; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0019] Example 2 The present embodiment provides a high-strength particle board, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 30%, add sodium hydroxide to adjust the solution pH to 12, stir at 40°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 50°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: After the wood chips with a moisture content of 4% were crushed, they were immersed in a 6% sodium hydroxide solution for 10 min, washed and dried, added to anhydrous ethanol and ultrasonically dispersed for 20 min, and then silane coupling agent and oxidized corn starch were added and stirred and mixed. The stirring speed was 200 r / min, the stirring time was 1 h, and the mixture was allowed to stand for 20 min after stirring. The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20:30:0.2:0.5; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 190°C, the pre-pressing time is 25 minutes, and the pre-pressing pressure is 2MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 110°C, the hot pressing time is 8 minutes, and the hot pressing pressure is 2MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0020] Example 3 The present embodiment provides a high-strength particle board, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 12:0.2; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 32%, add sodium hydroxide to adjust the solution pH to 12, stir at 46°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 60°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: wood chips with a moisture content of 5% were crushed and immersed in a sodium hydroxide solution with a mass concentration of 8% for 15 minutes, then washed and dried, added to anhydrous ethanol and ultrasonically dispersed for 30 minutes, and then silane coupling agent and oxidized corn starch were added and stirred and mixed. The stirring speed was 240 r / min, the stirring time was 1.2 hours, and the mixture was allowed to stand for 30 minutes after stirring. The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20:40:0.4:1; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing modified wood particles and an adhesive, paving the particles in a mold, pre-pressing the paved plate, the pre-pressing temperature is 200°C, the pre-pressing time is 35 minutes, and the pre-pressing pressure is 3MPa; then hot pressing and cooling, hot pressing the formed plate blank; the hot pressing temperature is 120°C, the hot pressing time is 10 minutes, and the hot pressing pressure is 3MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0021] Example 4 The present embodiment provides a high-strength particle board, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.2; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 30%, add sodium hydroxide to adjust the solution pH to 12, stir at 46°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 50°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: crush wood chips with a moisture content of 5%, soak them in a 6% sodium hydroxide solution for 15 minutes, wash and dry them, add them to anhydrous ethanol and ultrasonically disperse them for 20 minutes, then add silane coupling agent and oxidized corn starch and stir and mix them. The stirring speed is 240 r / min and the stirring time is 1 hour. After stirring, let it stand for 30 minutes. The weight ratio of wood chips, anhydrous ethanol, coupling agent and oxidized corn starch is 20:30:0.4:0.5; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 190°C, the pre-pressing time is 35 minutes, and the pre-pressing pressure is 2MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 120°C, the hot pressing time is 8 minutes, and the hot pressing pressure is 3MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0022] Comparative Example 1 This comparative example provides a high-strength particleboard, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 31%, add sodium hydroxide to adjust the solution pH to 12, stir at 43°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 55°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: wood chips with a moisture content of 4.5% were crushed and immersed in a 7% sodium hydroxide solution for 12 minutes, then washed and dried, added to anhydrous ethanol for ultrasonic dispersion for 25 minutes, and then isopropyl trioleate titanate and oxidized corn starch were added and stirred and mixed. The stirring speed was 220 r / min, the stirring time was 1.1 h, and the mixture was allowed to stand for 25 minutes after stirring. The weight ratio of wood chips, anhydrous ethanol, isopropyl trioleyl titanate and oxidized corn starch is 20:35:0.3:0.7; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0023] Comparative Example 2 This comparative example provides a high-strength particleboard, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 31%, add sodium hydroxide to adjust the solution pH to 12, stir at 43°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 55°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: wood chips with a moisture content of 4.5% were crushed and immersed in a 7% sodium hydroxide solution for 12 min, then washed and dried, added to anhydrous ethanol for ultrasonic dispersion for 25 min, and then oxidized corn starch was added and stirred at a speed of 220 r / min for 1.1 h. After stirring, the mixture was allowed to stand for 25 min. The weight ratio of wood shavings, anhydrous ethanol and oxidized corn starch is 20:35:0.7; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0024] Comparative Example 3 This comparative example provides a high-strength particleboard, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 31%, add sodium hydroxide to adjust the solution pH to 12, stir at 43°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 55°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: Wood chips with a moisture content of 4.5% were crushed, added to anhydrous ethanol and ultrasonically dispersed for 25 min, and then silane coupling agent and oxidized corn starch were added and stirred. The stirring speed was 220 r / min, the stirring time was 1.1 h, and the mixture was allowed to stand for 25 min after stirring. The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20:35:0.3:0.7; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0025] Comparative Example 4 This comparative example provides a high-strength particleboard, comprising corn starch modified particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of corn starch modified wood chips includes: crushing wood chips with a moisture content of 4.5%, soaking them in a sodium hydroxide solution with a mass concentration of 7% for 12 minutes, washing and drying them, adding them to anhydrous ethanol for ultrasonic dispersion for 25 minutes, then adding a silane coupling agent and corn starch and stirring and mixing them, the stirring and mixing speed is 220r / min, the stirring and mixing time is 1.1h, and standing for 25 minutes after stirring to obtain the obtained wood chips; The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and corn starch is 20:35:0.3:0.7; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the modified wood particles and the adhesive, paving them in a mold, pre-pressing the paved board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0026] Comparative Example 5 This comparative example provides a high-strength particle board, comprising corn starch, a particle composite and a urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The corn starch and wood shavings composite comprises wood shavings, anhydrous ethanol, a silane coupling agent and oxidized corn starch in a weight ratio of 20:35:0.3:0.7; The preparation method of oxidized corn starch is as follows: deionized water is added to corn starch to form a starch mixture with a mass ratio of 31%, sodium hydroxide is added to the solution to a pH of 12, potassium permanganate is added at a temperature of 43°C and stirred to a consistency with the starch content, sulfuric acid is added at a consistency with the starch content while maintaining a constant temperature, and the solution is washed and filtered when it turns pure white, and dried at a temperature of 55°C to obtain the oxidized corn starch; The preparation method of this high-strength particle board comprises the following steps: mixing corn starch, a particle compound and an adhesive, laying them in a mold, pre-pressing the laid and formed board, the pre-pressing temperature is 195° C., the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5 MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115° C., the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5 MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0027] Comparative Example 6 In this comparative example, a high-strength particleboard is provided, comprising particles and urea-formaldehyde resin adhesive in a weight ratio of 10:0.1; The preparation method of this high-strength particle board comprises the following steps: stirring and mixing the wood chips and the adhesive, laying them in a mold, pre-pressing the laid and formed board, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed board blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0028] Comparative Example 7 In this comparative example, a high-strength particle board is provided, which is corn starch modified particle board; The preparation method of corn starch modified wood chips comprises: (1) Preparation of oxidized corn starch: Add deionized water to corn starch to form a starch mixture with a mass ratio of 31%, add sodium hydroxide to adjust the solution pH to 12, stir at 43°C and add potassium permanganate in accordance with the starch content, keep the temperature constant, add sulfuric acid in accordance with the starch content, wash and filter when the solution turns pure white, and dry at 55°C to obtain the oxidized corn starch; (2) Preparation of corn starch modified wood chips: wood chips with a moisture content of 4.5% were crushed and immersed in a 7% sodium hydroxide solution for 12 minutes, then washed and dried, added to anhydrous ethanol and ultrasonically dispersed for 25 minutes, and then silane coupling agent and oxidized corn starch were added and stirred and mixed. The stirring speed was 220 r / min, the stirring time was 1.1 h, and the mixture was allowed to stand for 25 minutes after stirring. The weight ratio of wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20:35:0.3:0.7; The preparation method of the high-strength particle board comprises the following steps: laying the modified wood chips in a mold, pre-pressing the laid plate, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed plate blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0029] Comparative Example 8 This comparative example provides a high-strength particle board, which is a composite of corn starch and wood particles; The corn starch and wood shavings composite comprises wood shavings, anhydrous ethanol, a silane coupling agent and oxidized corn starch in a weight ratio of 20:35:0.3:0.7; The preparation method of oxidized corn starch is as follows: deionized water is added to corn starch to form a starch mixture with a mass ratio of 31%, sodium hydroxide is added to the solution to a pH of 12, potassium permanganate is added at a temperature of 43°C and stirred to a consistency with the starch content, sulfuric acid is added at a consistency with the starch content while maintaining a constant temperature, and the solution is washed and filtered when it turns pure white, and dried at a temperature of 55°C to obtain the oxidized corn starch; The preparation method of the high-strength particle board comprises the following steps: mixing corn starch and particle composite material, laying them in a mold, pre-pressing the laid plate, the pre-pressing temperature is 195°C, the pre-pressing time is 30 minutes, and the pre-pressing pressure is 2.5MPa; then hot pressing and cooling, hot pressing the formed plate blank; the hot pressing temperature is 115°C, the hot pressing time is 9 minutes, and the hot pressing pressure is 2.5MPa; then edge trimming and sanding are performed to obtain the high-strength particle board.
[0030] Test Example 1: The high-strength particleboard (with a thickness of 10 mm) prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 was subjected to the following tests: Water absorption expansion rate, mechanical properties: The mechanical properties of particleboard are tested with reference to GB / T4897-2015 "Particleboard" standard.
[0031] The results are shown in Table 1 below: Table 1
[0032] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength particleboard, It is characterized in that The invention comprises corn starch modified wood chips and an adhesive in a weight ratio of (10-12): (0.1-0.2); The preparation method of the corn starch modified wood chips comprises: crushing the wood chips, soaking them in sodium hydroxide solution, washing and drying them, adding them into anhydrous ethanol for ultrasonic dispersion, and then adding a silane coupling agent and oxidized corn starch and stirring and mixing them.
2. A high-strength particleboard according to claim 1, It is characterized in that The moisture content of the wood chips is 4%-5%, the mass concentration of the sodium hydroxide solution is 6%-8%, and the immersion time is 10-15 minutes.
3. A high-strength particleboard according to claim 1, It is characterized in that The ultrasonic dispersion time is 20-30 min.
4. The high-strength particleboard according to claim 1, It is characterized in that The stirring and mixing speed is 200-240r / min, the stirring and mixing time is 1-1.2h, and the mixture is allowed to stand for 20-30min after stirring.
5. The high-strength particleboard according to claim 1, It is characterized in that The weight ratio of the wood chips, anhydrous ethanol, silane coupling agent and oxidized corn starch is 20: (30-40): (0.2-0.4): (0.5-1).
6. The high-strength particleboard according to claim 1, It is characterized in that The preparation method of the oxidized corn starch comprises: adding deionized water to corn starch to form a starch mixed solution with a mass ratio of 30%-32%, adding sodium hydroxide to condition the solution to have a pH of 12, stirring at a temperature of 40-46° C. and adding potassium permanganate consistent with the starch content, keeping the temperature constant, adding sulfuric acid consistent with the starch content, washing and filtering when the solution turns pure white, and drying at a temperature of 50-60° C. to obtain the oxidized corn starch.
7. The high-strength particleboard according to claim 1, It is characterized in that The adhesive is urea-formaldehyde resin adhesive.
8. A method for preparing a high-strength particleboard according to any one of claims 1 to 7, It is characterized in that the steps include: The modified wood chips and adhesive are mixed and spread in a mold, the spread-formed board is pre-pressed, and then hot-pressed and cooled, and the hot-pressed board is trimmed and sanded to obtain the board.
9. A method for preparing a high-strength particleboard according to claim 8, It is characterized in that The pre-pressing temperature is 190-200° C., the pre-pressing time is 25-35 min, and the pre-pressing pressure is 2-3 MPa.