Rapid cleaning-free lightweight concrete production method and lightweight concrete

By mixing lightweight coarse aggregate and mortar in the mixing drum of a mixer truck, and then using a belt conveyor for conveying and fixed bagging, the problem of mixing lightweight coarse aggregate into conventional concrete has been solved, achieving efficient and safe production of lightweight concrete.

CN118927409APending Publication Date: 2024-11-12SHANGHAI CAIBA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299954.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing technologies, lightweight coarse aggregates are easily mixed in during conventional concrete production, resulting in low production efficiency, high equipment usage, material waste, and potential quality risks.

Method used

Pre-wetted lightweight coarse aggregate is mixed with mortar in the mixing drum of a mixer truck, conveyed by a belt conveyor and bagged to avoid working at heights and ensure the uniformity and production efficiency of lightweight concrete.

Benefits of technology

It improved production efficiency, reduced equipment usage, avoided potential quality problems, and ensured the uniformity and safety of concrete quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a rapid cleaning-free lightweight concrete production method and lightweight concrete. The production method sequentially comprises the steps that lightweight coarse aggregate in a non-waterproof bag is wetted and subjected to standing till the saturated surface is dry; 300-350 parts by mass of light coarse aggregate is put into a mixing drum of a mixer truck; 850-900 parts by mass of fine aggregate, 180-240 parts by mass of cement, 120-160 parts by mass of fly ash, 30-60 parts by mass of mineral powder and 160-200 parts by mass of water are weighed and put into a stirrer to be stirred into mortar; and uniformly mixing the mortar with the light coarse aggregate in a mixing drum of the mixer truck to finish the production of the light concrete. The lightweight concrete provided by the invention is prepared by adopting the production method. According to the lightweight concrete production method, the processes of cleaning the aggregate storage bin and cleaning the stirrer can be omitted, the production efficiency is improved, the equipment occupation condition is reduced, and the quality dispute caused by mixing the lightweight aggregate into the conventional concrete is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a rapid warehouse-clearance-free lightweight concrete production method and lightweight concrete. Background Art

[0002] Lightweight concrete is an important material for advocating energy-saving and environmentally friendly green buildings. It has significant economic benefits and ecological advantages, and can improve the thermal insulation effect of buildings to a certain extent and reduce energy consumption. At present, more and more buildings are using lightweight concrete for structural insulation, abandoning the original foam benzene board, aerated blocks and other insulation materials. In addition to the same characteristics of light weight and good thermal insulation effect, it also has the characteristics of good fire resistance, good impermeability and strong construction adaptability.

[0003] Mixing stations for producing concrete are usually equipped with aggregate bins to store aggregates used in producing concrete. Since the aggregate used in lightweight concrete is lightweight coarse aggregate, there will often be residual lightweight coarse aggregate in the aggregate bins that have stored lightweight coarse aggregate and the mixers that have mixed lightweight coarse aggregate. When producing conventional concrete, if the lightweight coarse aggregate left in the aggregate bins and mixers is mixed into conventional concrete, the conventional concrete will float on the construction site or form a weak structural area, resulting in quality risks. In order to avoid this quality risk, it is usually necessary to clean the aggregate bins that have stored lightweight coarse aggregate and the mixers that have mixed lightweight coarse aggregate after manufacturing lightweight concrete, resulting in low production efficiency of lightweight concrete; or in the process of manufacturing lightweight concrete, the lightweight coarse aggregate is directly shoveled into the mixer truck using a forklift, which not only requires an additional forklift equipment in the production process of lightweight concrete, but also easily spills out of the mixer truck, resulting in waste of production materials. Summary of the invention

[0004] In view of the defects existing in the prior art, the present application provides a method for producing lightweight concrete without clearing warehouse and lightweight concrete, so as to solve the technical problems in the prior art of avoiding mixing lightweight coarse aggregate into conventional concrete, resulting in low production efficiency or more equipment occupied, and easy waste of production materials.

[0005] In order to achieve the purpose of the above invention, the technical solution provided by the present invention is as follows:

[0006] A method for producing lightweight concrete quickly and without warehouse clearance comprises the following steps:

[0007] S1. Wetting the lightweight coarse aggregate and leaving it to stand until it reaches a saturated surface dry state, wherein the lightweight coarse aggregate is bagged in a non-waterproof storage bag according to a fixed weight;

[0008] S2. Place 300-350 parts by mass of lightweight coarse aggregate that has reached saturated surface dryness into the mixing drum of a mixer truck;

[0009] S3, weighing 850-900 parts of fine aggregate, 180-240 parts of cement, 120-160 parts of fly ash, 30-60 parts of mineral powder, and 160-200 parts of water by mass into a mixer and mixing into mortar;

[0010] S4, driving the mixer truck in S2 to the mixer discharge port to load mortar, and mixing the lightweight coarse aggregate and mortar in the mixing barrel of the mixer truck until the lightweight coarse aggregate and mortar are evenly mixed, thereby completing the production of lightweight concrete.

[0011] In one embodiment, the lightweight coarse aggregate is ceramsite.

[0012] In one embodiment, the ceramsite is a saturated surface dry 5-25 mm continuously graded ceramsite, and the density of the ceramsite is 300-400 kg / m 3 , cylinder pressure strength ≥1.0MPa.

[0013] In one embodiment, in step S2 , the lightweight coarse aggregate is conveyed into the mixing drum of the mixer truck by a belt conveyor, wherein the belt conveyor is used to specifically convey the lightweight coarse aggregate.

[0014] In one embodiment, a groove is fixedly provided on the belt of the belt conveyor.

[0015] In one embodiment, the belt conveyor is provided with rollers.

[0016] In one embodiment, step S1 specifically includes watering and moistening the lightweight coarse aggregate in the woven bag for a period of time, and then covering the woven bag with a waterproof cloth to allow it to dry naturally in the shade to a saturated surface dry state, wherein the watering time is 3-5 hours and the shade drying time is 3-5 hours.

[0017] In one embodiment, the fine aggregate is machine-made medium sand, the cement is P.O42.5 cement, the fly ash is secondary high-calcium ash, and the mineral powder is S95 mineral powder.

[0018] This embodiment also provides a fast, clean-out-free lightweight concrete, which is produced by the fast, clean-out-free lightweight concrete production method. The lightweight concrete is a structural thermal insulation lightweight aggregate concrete with a maximum strength grade of LC7.5 and LC5.0.

[0019] Compared with the prior art, this application has at least the following beneficial effects:

[0020] The fast and clean-out-free lightweight concrete production method of the present invention directly puts lightweight coarse aggregate into the mixing drum of a mixer truck, and then puts the mortar in the mixer into the mixing drum of the mixer truck, and completes the production of lightweight concrete in the mixing drum, eliminating the need to clean the aggregate bin and the mixer, thereby improving production efficiency, reducing equipment occupancy, and avoiding quality disputes caused by lightweight aggregate mixed into conventional concrete. The mixing station can produce lightweight concrete and ordinary concrete at the same time without clearing the warehouse and cleaning the mixer, thereby accelerating the production rhythm and expanding the production scope.

[0021] The present invention uses a special belt conveyor to convey a certain mass of lightweight coarse bones that have reached saturated surface dryness to the mixing drum of the mixer truck, avoiding high-altitude operations at the entrance of the mixing drum and improving the safety of operation; the belt of the belt conveyor is fixedly provided with a groove to reduce the sliding and lateral movement of the ceramsite, prevent the tumbling, loss and accumulation of the ceramsite, effectively improve the conveying efficiency, and facilitate measurement; the belt conveyor is equipped with rollers, which is convenient for movement and reduces space occupation, is suitable for mixing stations with smaller sites, and is conducive to equipment maintenance. Compared with a fixed belt conveyor that requires the mixer truck to accurately reverse so that the receiving hopper is aligned with the belt conveyor, the mobile belt conveyor is equipped with rollers that can move the belt conveyor to the mixing truck receiving hopper, thereby avoiding the problem of time and labor consumption caused by the mixer truck reversing without aligning the belt conveyor;

[0022] The present application adopts pre-wetted saturated surface-dry lightweight coarse aggregate to prevent the lightweight coarse aggregate from sticking together and absorbing mixing water during the mixing process due to failure to pre-wet, resulting in uncontrollable water consumption, thereby ensuring the uniformity and stability of the concrete quality. The lightweight coarse aggregate is bagged according to a fixed weight and can be directly added according to the production volume without weighing, which is convenient for measurement and improves production efficiency.

[0023] The present application adopts the method of loading lightweight coarse aggregate into the mixing drum and then loading mortar, making full use of the characteristic that lightweight coarse aggregate is easy to float in concrete, so that the lightweight coarse aggregate can be fully and evenly mixed with the mortar in the mixing drum, thereby ensuring the quality of lightweight concrete. DETAILED DESCRIPTION

[0024] In the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessarily obscuring the concepts of the present invention.

[0025] The terms used in this disclosure are for the purpose of describing specific embodiments only and are not intended to limit the disclosure. The singular forms of "a", "said" and "the" used in this disclosure and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0026] It should be understood that although the terms first, second, third, etc. may be used in the present disclosure to describe various information, such information should not be limited to these terms and should not be understood as indicating or implying relative importance. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present disclosure, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Depending on the context, the word "if" as used herein may be interpreted as "at the time of" or "when" or "in response to determining".

[0027] In the description of the present invention, unless otherwise specified and limited, it should be noted that the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a mechanical connection or the internal connection between two components. It can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to the specific circumstances.

[0028] A specific embodiment provides a method for producing lightweight concrete quickly without warehouse clearance, comprising the following steps:

[0029] S1. Wet the lightweight coarse aggregate packed in non-waterproof woven bags according to fixed weight and let it stand until it is saturated and dry. The lightweight coarse aggregate is ceramsite, which is saturated and dry 5-25mm continuous graded ceramsite with a density of 300-400kg / m 3 , cylinder pressure strength ≥1.0MPa;

[0030] S2. 300-350 parts by weight of lightweight coarse aggregate that has reached saturated surface dryness are placed into the mixing drum of the mixer truck through a belt conveyor, wherein the belt conveyor is used to transport the lightweight coarse aggregate;

[0031] S3. 850-900 parts of fine aggregate, 180-240 parts of cement, 120-160 parts of fly ash, 30-60 parts of mineral powder and 160-200 parts of water are weighed by mass and put into a mixer and stirred into mortar, wherein the fine aggregate is machine-made medium sand, the cement is P.O42.5 cement, the fly ash is secondary high calcium ash, and the mineral powder is S95 mineral powder;

[0032] S4, driving the mixer truck in S2 to the mixer discharge port to load mortar, and mixing the lightweight coarse aggregate and mortar in the mixing barrel of the mixer truck until the lightweight coarse aggregate and mortar are evenly mixed, thereby completing the production of lightweight concrete.

[0033] Specifically, step S1 specifically includes watering and moistening the lightweight coarse aggregate in the woven bag for a period of time, and then covering the woven bag with a waterproof cloth to allow it to dry naturally in the shade to a saturated surface dry state, wherein the watering time is 3-5 hours, and the shade drying time is 3-5 hours.

[0034] Specifically, a groove is fixedly provided on the belt of the belt conveyor. Through the setting of the belt conveyor, the lightweight coarse aggregate is transported from a low place to the entrance of the mixing drum of the mixer, avoiding the high-altitude operation of putting materials into the mixing drum of the mixer. Because ceramsite is a round particle, a groove is fixedly provided on the belt to prevent the ceramsite from rolling and ensure the quality of the ceramsite entering the mixing drum.

[0035] The specific implementation method provides a fast and clean-free lightweight concrete, which is produced by the fast and clean-free lightweight concrete production method. The lightweight concrete is a structural thermal insulation lightweight aggregate concrete with the highest strength grade of LC7.5 and LC5.0.

[0036] In order to better understand the scheme of the present invention, the following group of embodiments and a group of comparative examples are provided for illustration:

[0037] Example:

[0038] S1. According to the mass ratio, 300 parts of 5-25 mm ceramsite packed in non-waterproof woven bags according to a fixed weight are watered for four hours to moisten them, and covered with waterproof cloth for four hours until the ceramsite is naturally dried in the shade to a saturated surface dry state;

[0039] S2, conveying the ceramsite to the mixing drum of the mixer truck through a special belt conveyor;

[0040] S3, a mixer weighs 880 parts of fine aggregate, 220 parts of cement, 160 parts of water, 120 parts of fly ash, and 60 parts of mineral powder according to the mass fraction ratio and mixes them into mortar;

[0041] S4. Load the mortar into the mixer truck already loaded with expanded clay, and quickly reverse it until it is uniform, so as to obtain lightweight concrete of LC7.5. After the lightweight concrete is delivered to the construction site, the mixer truck returns to the station to clean the mixing drum to prevent expanded clay from entering the conventional concrete.

[0042] Comparative Example:

[0043] S1. First, water the 5-25mm ceramsite for four hours to moisten it, and cover it with a waterproof cloth for four hours until the ceramsite is naturally dried in the shade to a saturated surface dry state;

[0044] S2. Clear the coarse aggregate bin in the mixing station and place the saturated surface-dried ceramsite in S1 into the coarse aggregate bin;

[0045] S3. According to the mass ratio, 300 parts of ceramsite, 880 parts of fine aggregate, 220 parts of cement, 160 parts of water, 120 parts of fly ash, and 60 parts of mineral powder were weighed and put into a mixer for uniform mixing to obtain a lightweight concrete of LC7.5, which was then loaded into a mixer truck;

[0046] S4. After production is completed, the aggregate bin is cleared and the mixer is cleaned. After the lightweight concrete is delivered to the construction site, the mixer truck returns to the station to clean the mixing drum to prevent expanded clay from entering the conventional concrete.

[0047] The examples and comparative examples were tested for strength according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the dry apparent density was tested according to JGJ51-2002 "Technical Specifications for Lightweight Aggregate Concrete", as well as the comparison of production processes.

[0048] Group Compressive strength / MPa <![CDATA[Dry apparent density / kg / m 3 > Cleaning Example 8.0 1730 Mixer Truck Comparative Example 7.9 1740 Aggregate silo, mixer, mixer truck

[0049] It can be seen from the performance test that the embodiment and the comparative example are basically the same in compressive strength and dry apparent density. However, compared with the comparative example, the embodiment only needs to clean the mixer truck in the cleaning link, and the aggregate silo and mixer are not cleaned, which greatly reduces the quality risk of lightweight aggregate mixed into conventional concrete. At the same time, since there is no link of cleaning the aggregate silo and mixer, not only the production time is shortened, but also the production of conventional concrete will not be affected, which is extremely beneficial for ordinary mixing plants.

[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A method for producing lightweight concrete quickly and without warehouse clearance. It is characterized in that The following steps are involved: S1. Wetting the lightweight coarse aggregate and leaving it to stand until it reaches a saturated surface dry state, wherein the lightweight coarse aggregate is bagged in a non-waterproof storage bag according to a fixed weight; S2. Place 300-350 parts by mass of lightweight coarse aggregate that has reached saturated surface dryness into the mixing drum of a mixer truck; S3, weighing 850-900 parts of fine aggregate, 180-240 parts of cement, 120-160 parts of fly ash, 30-60 parts of mineral powder, and 160-200 parts of water by mass into a mixer and mixing into mortar; S4, driving the mixer truck in S2 to the mixer discharge port to load mortar, and mixing the lightweight coarse aggregate and mortar in the mixing barrel of the mixer truck until the lightweight coarse aggregate and mortar are evenly mixed, thereby completing the production of lightweight concrete.

2. The method for producing lightweight concrete without requiring cleaning as claimed in claim 1, It is characterized in that The lightweight coarse aggregate is ceramsite.

3. The method for producing lightweight concrete without warehouse clearance as claimed in claim 2, It is characterized in that The ceramsite is a saturated surface dry 5-25mm continuously graded ceramsite, and the density of the ceramsite is 300-400kg / m 3 , cylinder pressure strength ≥1.0MPa.

4. The method for producing lightweight concrete without requiring cleaning as claimed in claim 1, It is characterized in that In step S2, the lightweight coarse aggregate is conveyed into the mixing drum of the mixer truck by a belt conveyor, wherein the belt conveyor is used to specifically convey the lightweight coarse aggregate.

5. The method for producing lightweight concrete without requiring cleaning as claimed in claim 4, It is characterized in that A groove is fixedly arranged on the belt of the belt conveyor.

6. The method for producing lightweight concrete without requiring cleaning as claimed in claim 4, It is characterized in that The belt conveyor is provided with rollers.

7. The method for producing lightweight concrete without requiring cleaning as claimed in claim 1, It is characterized in that Step S1 specifically includes watering and moistening the lightweight coarse aggregate in the woven bag for a period of time, and then covering the woven bag with a waterproof cloth to allow it to dry naturally in the shade until it reaches a saturated surface dry state, wherein the watering time is 3-5 hours and the shade drying time is 3-5 hours.

8. The method for producing lightweight concrete without requiring cleaning as claimed in claim 1, It is characterized in that The fine aggregate is machine-made medium sand, the cement is P.O42.5 cement, the fly ash is secondary high-calcium ash, and the mineral powder is S95 mineral powder.

9. A lightweight concrete, It is characterized in that The lightweight concrete is produced by the rapid clearance-free lightweight concrete production method as described in any one of claims 1 to 8, and the lightweight concrete is a structural thermal insulation lightweight aggregate concrete with a maximum strength grade of LC7.5 or LC5.0.