Method and system for manufacturing large-aperture diaphragm by using mixed oil instead of inorganic filler
By replacing the inorganic filler with mixed oil, large-pore diaphragm is prepared by extrusion molding and gas-solid separation treatment, the problems of insufficient base film strength and uneven pore size in the prior art are solved, and the production of high-strength and uniform pore size is achieved.
Patent Information
- Application Number
- CN202410989179.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing large-pore PE base films are insufficient in production due to the addition of inorganic fillers and the pore size is uneven, which cannot meet the high pressure environment and high throughput requirements.
Mixed oil instead of inorganic fillers, large pore size membranes are prepared through extrusion molding, gas-solid separation treatment and post-treatment steps. Using a combination of volatile and non-volatile oils, porous membranes are formed by negative pressure stretching, and through extraction and Drying gives a uniform pore size membrane.
The uniformity and high strength of the large-pore diaphragm are achieved, suitable for high-pressure environments, the needle puncture strength and tensile strength are significantly improved, and the pore diameter uniformity is improved, solving the problems of too low base film strength and uneven pore diameter.
Smart Images

Figure CN118927653A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of diaphragm technology, and in particular to a method and device for manufacturing a large-aperture diaphragm by replacing inorganic fillers with mixed oil. Background Art
[0002] Currently, various industries, including biomedical filtration, front-end filtration of water treatment, and front-end processing of semiconductor chemical reagents, have an increasing demand for diaphragms with large pore size, high flux, and low barrier properties. This includes the preparation of solid electrolytes in the field of solid-state batteries, and the use of polymers to improve their strength and ionic conductivity.
[0003] Since nowadays, large-pore PE base membranes are mainly used for water treatment base membranes or medical supplies. The idea of existing large-pore base membranes is to mix inorganic fillers into the powder, and use the inorganic fillers to expand the pore size during the stretching of the base membrane. The base membrane formed by this stretching method will form a small hole next to the large pore while forming a large pore, so when measuring the narrow pore size distribution, there will be two pore size distribution peaks, one large and one small. In addition, since the large-pore base membrane has a high pore size and high porosity, the strength of the base membrane itself is slightly weak, and the inorganic fillers added during production further weaken the strength of the base membrane. Therefore, it is not suitable for high-pressure production environments.
[0004] Therefore, there is an urgent need for a diaphragm that does not use inorganic fillers to prevent the base membrane from being too weak and can make the pore size more uniform to solve the problem of uneven pore size of the base membrane. Summary of the invention
[0005] Therefore, the main purpose of the present application is to provide a method and device for manufacturing a large-pore diaphragm by replacing inorganic fillers with mixed oil, so as to further optimize the above-mentioned problems.
[0006] In order to solve the above technical problems, the purpose of the present application is to provide a method for manufacturing a large-pore diaphragm by replacing inorganic filler with mixed oil, which is characterized in that it includes the following steps: an extrusion molding step: the plastic material and the mixed oil are melt-extruded through an extruder to obtain a casting, wherein the mixed oil contains a volatile oil product and a non-volatile oil product; an oil-gas volatilization step: the casting is subjected to a gas-solid separation treatment so that the oil and gas volatilized from the volatile oil product in the mixed oil leave the casting to obtain a porous membrane; and a post-treatment step: the porous membrane is extracted and dried to obtain a large-pore diaphragm.
[0007] The method as described above further comprises: a mixing step: mixing the volatile oil product and the non-volatile oil product to obtain the mixed oil.
[0008] In the above method, the gas-solid separation process includes utilizing negative pressure to volatilize the volatile oil in the casting into the oil gas so as to leave the casting.
[0009] In the above method, the gas-solid separation treatment includes: a stretching volatilization step: the obtained casting is stretched so that the volatile oil in the casting is volatilized into the oil gas to leave the casting.
[0010] As described above, the stretching and volatilization step further includes the following steps: a negative pressure stretching step: stretching the cast sheet under a negative pressure environment so that the volatile oil volatilizes from the cast sheet to form a plurality of micropores on the cast sheet; and an expansion stretching step: stretching the cast sheet again to further expand the micropores to form the porous membrane.
[0011] In the method as described above, the post-processing step includes: an extraction step: subjecting the porous membrane to an extraction treatment to clean off the non-volatile oil product to form an extraction membrane; and a drying step: subjecting the extraction membrane to a drying treatment to obtain a large pore size diaphragm.
[0012] The method as described above further comprises the following steps: an oil and gas recovery step: recovering the oil and gas formed by the volatilization of the volatile oil product in the stretching volatilization step.
[0013] As described above, the volatile oil product comprises normal, isomeric or cycloparaffin C6 mineral oil, the non-volatile oil product comprises white oil, and the plastic material comprises polyethylene.
[0014] In the above method, the ratio between the volatile oil and the non-volatile oil is 1:(0.1-0.2).
[0015] In the above method, in the stretching volatilization step, the negative pressure condition ranges from -500 Pa to -100 Pa relative to atmospheric pressure.
[0016] Another object of the present application is to provide a large-pore diaphragm prepared by the method of using mixed oil to replace inorganic filler to prepare a large-pore diaphragm as described above, characterized in that the maximum pore size of the large-pore diaphragm is between 85nm~100nm.
[0017] The large-pore diaphragm as described above, wherein the needle puncture strength of the large-pore diaphragm is greater than 80gf / μm, and the MD tensile strength of the large-pore diaphragm is greater than 800kgf / cm 2 The TD tensile strength of the large-aperture diaphragm is greater than 800 kgf / cm 2 The large-pore diaphragm has an MD elongation greater than 50% and a TD elongation greater than 50%.
[0018] Another object of the present application is to provide a system for manufacturing a large-aperture diaphragm by replacing inorganic fillers with mixed oil. The invention is characterized in that it comprises: a mixer for mixing a volatile oil product and a non-volatile oil product to obtain a mixed oil; an extruder for melting and extruding a plastic material and the mixed oil through the extruder to obtain a casting sheet; a protective cover surrounding the extrusion die head of the extruder to confine the volatilization space of the volatile oil product in the casting sheet within the protective cover, thereby preventing the volatile oil product from diffusing and volatilizing into an open environment; a stretching volatilization device for stretching the obtained casting sheet to volatilize the volatile oil product to obtain a porous membrane; an extraction device for extracting the porous membrane to wash away the non-volatile oil product to form an extraction membrane; and a drying device for drying the extraction membrane to obtain a large-pore diameter diaphragm.
[0019] In the system as described above, the stretching and volatilization device further comprises: a negative pressure stretching device for stretching the casting sheet under a negative pressure environment so that the volatile oil volatilizes from the casting sheet to form a plurality of micropores on the casting sheet; and an expansion stretching device for stretching the casting sheet again to further expand the micropores to form the porous membrane.
[0020] The system as described above further comprises: an oil gas recovery device for recovering the oil gas generated by the volatilization of the volatile oil product.
[0021] The present invention prepares a method for making a large-aperture diaphragm by replacing inorganic fillers with mixed oil, which is similar to the manufacturing process of lithium battery base membrane. No inorganic fillers need to be added to the raw materials. Since the addition of inorganic fillers will further reduce the strength of the base membrane, the present invention without adding inorganic fillers can solve the problem of low base membrane strength in the prior art. In addition, the production of traditional large-aperture membrane base membranes will form small holes next to the large holes, and there are fewer effective large holes, and the use effect is not ideal. The membrane making process of the present invention is similar to the process of wet-process diaphragms, so it can make the pore size more uniform and solve the problem of uneven pore size of the base membrane. Therefore, the present invention is suitable for increasing the pore size and porosity of the base membrane, and at the same time improving the strength of the base membrane to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic block diagram of a process for producing a large-pore diaphragm by replacing an inorganic filler with a mixed oil according to an embodiment of the present application.
[0023] Figure 2 This is a flow block diagram of a method for producing a large-pore diaphragm by replacing inorganic filler with mixed oil according to another embodiment of the present application.
[0024] Figure 3 This is a schematic block diagram of a process for producing a large-pore diaphragm by replacing an inorganic filler with a mixed oil according to another embodiment of the present application.
[0025] Figure 4 This is a schematic block diagram of a process for producing a large-pore diaphragm by replacing an inorganic filler with a mixed oil according to another embodiment of the present application.
[0026] Figure 5 This is a schematic diagram of the device configuration of a system for manufacturing a large-pore diaphragm by replacing inorganic filler with mixed oil according to an embodiment of the present application.
[0027] Figure 6 This is a schematic diagram of the device configuration of a system for manufacturing a large-pore diaphragm by replacing inorganic filler with mixed oil according to another embodiment of the present application.
[0028] Figure 7 This is a schematic diagram of the device configuration of a system for manufacturing a large-pore diaphragm by replacing inorganic fillers with mixed oil according to another embodiment of the present application. DETAILED DESCRIPTION
[0029] The following descriptions of the embodiments refer to the attached drawings to illustrate specific embodiments that can be implemented in the present application. Directional terms mentioned in the present application, such as "upper", "lower", "front", "back", "left", "right", "inner", "Outside", "side", etc., are only used to refer to the directions of the attached drawings. Therefore, the directional terms used are used to explain and understand the present application, but not to limit the present application.
[0030] The accompanying drawings and descriptions are considered to be illustrative in nature and not restrictive. In the drawings, units with similar structures are represented by the same reference numerals. In addition, for the sake of understanding and ease of description, the size and thickness of each component shown in the drawings are arbitrarily shown, but the application is not limited thereto.
[0031] In the drawings, the thickness of layers, films, regions, etc. are exaggerated for clarity. In the drawings, the thickness of some layers and regions are exaggerated for understanding and ease of description. It will be understood that when a component such as a layer, film, region, or substrate is referred to as being "on" another component, the component may be directly on the other component, or intermediate components may also be present.
[0032] In addition, in the specification, unless explicitly described to the contrary, the word "comprising" will be understood to mean including the components, but not excluding any other components. In addition, in the specification, "on" means being located above or below the target component, and does not mean necessarily being located on the top based on the direction of gravity.
[0033] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of a low-barrier diaphragm and its preparation method proposed in the present application, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and specific embodiments.
[0034] A method 1 of using mixed oil to replace inorganic filler to make a large-aperture diaphragm in one embodiment of the present application, see Figure 1 , characterized in that it includes the following steps: a mixing step S11: mixing a volatile oil product and a non-volatile oil product to obtain a mixed oil; an extrusion molding step S12: melt-extrude the plastic material and the mixed oil through an extruder to obtain a casting, wherein the mixed oil contains a volatile oil product and a non-volatile oil product; an oil-gas volatilization step S13: subjecting the casting to a gas-solid separation treatment so that the oil and gas volatilized from the volatile oil product in the mixed oil leave the casting to obtain a porous membrane; a post-treatment step S14: extracting and drying the porous membrane to obtain a large-pore diameter diaphragm.
[0035] In some embodiments, the gas-solid separation process in the oil-gas volatilization step S13 includes using negative pressure to volatilize the volatile oil in the casting into the oil gas so as to leave the casting. In this embodiment, the gas-solid separation process includes: a stretching volatilization step: stretching the obtained casting so that the volatile oil in the casting volatilizes into the oil gas so as to leave the casting. In some embodiments, please refer to Figure 2 The post-processing step S14 includes: an extraction step S141: extracting the porous membrane to wash away the non-volatile oil to form an extraction membrane; and a drying step S142: drying the extraction membrane to obtain a large pore size membrane.
[0036] In some embodiments, see Figure 3, the method 1 of using mixed oil to replace inorganic filler to make a large-pore diaphragm, before the post-processing step S14, further comprises the following steps: a heat preservation step S15: heat preservation treatment of the porous membrane. In addition, the stretching and volatilization step in the oil and gas volatilization step S13 further comprises the following steps: a negative pressure stretching step S131: stretching the casting under a negative pressure environment so that the volatile oil volatilizes from the casting to form a plurality of micropores on the casting; and an expansion and stretching step S132: stretching the casting again to further expand the micropores to form the porous membrane.
[0037] See also Figure 4 In some embodiments, the method 1 for making a large-aperture diaphragm by replacing inorganic fillers with mixed oil further comprises the following steps when performing the oil and gas volatilization step S13: an oil and gas recovery step S16: recovering the oil and gas generated by the volatilization of the volatile oil product in the stretching volatilization step S13. However, it is not limited thereto, and the oil and gas recovery step S16 can also be started during the extrusion molding step S12, because at this time, some of the volatile oil products in the casting sheet have begun to volatilize, and the oil and gas recovery step S16 can not only prevent the volatile oil products from diffusing and volatilizing into an open environment to cause pollution, but also can reuse the recovered oil and gas.
[0038] In some embodiments, the volatile oil product comprises normal, isomeric or cycloparaffin C6 mineral oil, the non-volatile oil product comprises white oil, and the plastic material comprises polyethylene. In addition, in the mixing step S11, the ratio of the volatile oil product to the non-volatile oil product is 1:(0.1-0.2). In step S13, the negative pressure condition ranges from -500 Pa to -100 Pa relative to atmospheric pressure.
[0039] The main principle of the present invention is: similar to the wet diaphragm process, the white oil is replaced by a mixture of 10% white oil and 90% of a mineral oil with a certain volatility. The mineral oil is relatively slow in volatility to prevent it from volatilizing completely before entering the transverse stretching process. After entering the transverse stretching oven, the air flow rate inside the oven increases, and a negative pressure state needs to be formed in the oven to accelerate the volatilization of the mineral oil during the transverse stretching process. The steps described above volatilize the mineral oil, leaving micropores on the membrane, and then the micropores are further expanded by stretching. The non-volatile white oil allows the base membrane to still have a certain fluidity after losing the mineral oil, preventing the base membrane from breaking during the stretching process. Due to the use of volatile mineral oil, the entire extrusion and stretching process needs to ensure a fairly high degree of airtightness. It can be understood that in order to prevent the micropores from being stretched into a narrow and long shape, bidirectional synchronous stretching is required.
[0040] It is worth mentioning that in order to control the volatilization rate and prevent the mineral oil from volatilizing completely before extrusion. Therefore, a mineral oil with relatively low volatility is selected, and the volatility is increased by increasing the membrane surface area during the stretching process and in a negative pressure environment. Because mineral oil has a certain volatility and poses a safety hazard in an open environment, it is necessary to seal it with a cover starting from the extruder die head. The stretching of the present invention is divided into two times, and the volatilized mineral oil is between the two stretching processes. After the second stretching, the white oil extraction stage is entered. However, it does not need to be sealed during extraction, and it has basically evaporated during the negative pressure stretching. Therefore, the idea of the present invention is to mix a pore-forming agent with a certain volatility and another non-volatile pore-forming agent. During the stretching process, a part of the volatile pore-forming agent is evaporated to increase the pore size, and a part of the non-volatile pore-forming agent is retained to ensure the fluidity of the membrane during the stretching process.
[0041] In another embodiment, the present application provides a large-pore diaphragm prepared by the method 1 of using mixed oil to replace inorganic filler to prepare a large-pore diaphragm as described above, characterized in that the maximum pore size of the large-pore diaphragm is between 85nm and 100nm. The needle puncture strength of the large-pore diaphragm is greater than 80gf / μm, and the MD tensile strength of the large-pore diaphragm is greater than 800kgf / cm 2 The TD tensile strength of the large-aperture diaphragm is greater than 800 kgf / cm 2 The large-pore diaphragm has an MD elongation greater than 50% and a TD elongation greater than 50%.
[0042] In yet another embodiment, see Figure 5 The present application provides a system 2 for making a large-pore diaphragm by replacing inorganic fillers with a mixed oil, which comprises: a mixer 21 for mixing a volatile oil product with a non-volatile oil product to obtain a mixed oil; an extruder 22 for melting and extruding a plastic material and the mixed oil through an extruder to obtain a casting; a stretching volatilization device 23 for stretching the obtained casting and volatilizing the volatile oil product by negative pressure to obtain a porous membrane; an extraction device 24 for extracting the porous membrane and washing away the non-volatile oil product to form an extraction membrane; and a drying device 25 for drying the extraction membrane to obtain a large-pore diaphragm.
[0043] In some embodiments, see Figure 6 This system uses mixed oil instead of inorganic filler to make large-aperture diaphragm The stretching and volatilization device 23 further includes: a negative pressure stretching device 231, which is used to stretch the casting sheet under a negative pressure environment so that the volatile oil is volatilized from the casting sheet to form a plurality of micropores on the casting sheet; and an expansion stretching device 232, which is used to stretch the casting sheet again to further expand the micropores to form the porous membrane.
[0044] Also, see Figure 7 The system 2 for making a large-aperture diaphragm using mixed oil instead of inorganic filler further includes a protective cover 27 surrounding the extrusion die of the extruder 22, so as to confine the space for the volatile oil in the casting to volatilize within the protective cover 27, thereby preventing the volatile oil from diffusing and volatilizing to an open environment. It is understandable that the protective cover 27 can extend all the way to the stretching volatilization device 23 to form an integrated structure, so that the conveying path of the casting from the extrusion die of the extruder 22 to the feed inlet of the stretching volatilization device 23 is kept within the closed space of the protective cover 27, so as to effectively prevent the volatile oil from diffusing and volatilizing to an open environment to cause pollution.
[0045] In addition, an oil and gas recovery device 28 may be provided to recover the oil and gas generated by the volatilization of the volatile oil. It is worth mentioning that the oil and gas recovery device 28 may be integrated into the stretching volatilization device 23 and simultaneously connected to the space enclosed by the protective cover 27, so that the oil and gas generated by the cast sheet from the time it leaves the extrusion die of the extruder 22 to the stretching volatilization device 23 for stretching can be effectively recovered and reused.
[0046] The present invention intends to protect the use of mixed mineral oil to replace inorganic fillers to make large-aperture diaphragms, and is not limited to the type of oil and the proportion of the mixed ratio. The present invention uses a mixture of normal, isomeric and cycloalkane C6 mineral oil and white oil and co-extruded with polyethylene powder with a molecular weight of 400,000 to 600,000. After longitudinal stretching, as the film thickness becomes thinner and the surface area increases, a negative pressure device is added to make the mineral oil begin to volatilize in large quantities to form micropores, and the pore size is further expanded by longitudinal stretching. Since the copolymer formed by the mixed oil and PE forms micropores after the mineral oil volatilizes, the pores are further expanded by bidirectional synchronous stretching. Compared with using inorganic fillers, mineral oil has a better distribution effect and a more uniform pore size.
[0047] In the invention, some parameters are designed to conduct experiments, and the experimental process and results are summarized as follows.
[0048] This experiment simulates the extruder cast film by melting the raw materials in a reactor and then using a flat vulcanizer to die-cast the film. The biaxial stretching machine was then used to simulate the biaxial stretching of the production line. This experiment used dearomatized fluid D95, which has similar physical properties to mineral oil and petroleum solvents and has less impact on health and the environment during the volatilization process than mineral oil and petroleum solvents.
[0049] The first experiment (1#): 70 g of low-viscosity white oil was mixed with 30 g of PE with a molecular weight of 400,000;
[0050] The second experiment (2#): 7g of low viscosity white oil and 63g of dearomatized fluid D95 were mixed with 30g of molecular weight 40 10,000 PE mixed;
[0051] The third experiment (3#): 30 g of nano-alumina powder was mixed with 30 g of PE with a molecular weight of 400,000.
[0052] The three groups of mixed raw materials were placed in a reactor to fully melt, and 17g of the melt was taken from each reactor and pressed into a casting sheet with a thickness of 0.8mm using a flat vulcanizer. The sheets were then subjected to a bidirectional synchronous 8x*8x stretching on a bidirectional stretching machine. The temperature in the bidirectional stretching machine was 115°C. After the stretching was completed, the sheets were allowed to stay for 2 minutes to allow the 2# dearomatized fluid to fully evaporate. After stretching, 1# and 2# were tightened to the frame and the remaining white oil was extracted with dichloromethane. No white oil was added to 3#, so no extraction was required. 1# and 2# were placed on a frame to remove the remaining white oil. The pore size test and mechanical test data of the 3# base film sample are as follows: Table 1
[0053] The pore size can be further expanded through process conditions during production. Due to the large pore size and high porosity of macroporous membranes, the mechanical strength is generally weaker than that of conventional base membranes. The addition of 50% inorganic powder alumina to 3# further weakens the strength of the membrane and makes the elongation very low. If used in actual products, the membrane is very easy to break. 2# has better mechanical properties.
[0054] In summary, in order to solve the current problems of using inorganic fillers, the present invention adopts a method of not using inorganic fillers to prevent the base membrane strength from being too low. Since the base membrane itself has a large pore size and a high porosity, the strength of the base membrane is slightly lower if inorganic powder is added. The present invention is similar to the manufacturing process of the lithium battery base membrane, and no inorganic filler is required to be added to the raw materials. In addition, the present invention can also solve the problem of uneven base membrane pore size. Since the production of traditional macroporous membrane base membranes will form small holes next to the large holes, there are fewer effective large holes, and the use effect is not ideal. This membrane making process is similar to the process of wet diaphragms, which can make the pore size more uniform.
[0055] The phrase "in some embodiments" and "in various embodiments" is used repeatedly. The phrase generally does not refer to the same embodiment; however, it may refer to the same embodiment. The words "including," "having," and "comprising" are synonymous unless the context indicates otherwise.
[0056] The above description is only an embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application has been disclosed as above with specific embodiments, it is not intended to limit the present application. Any technician familiar with the profession can make slight changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present application. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. A method for making a large-aperture diaphragm by replacing inorganic filler with mixed oil. It is characterized in that The following steps are involved: An extrusion molding step: melt-extrude the plastic material and the mixed oil through an extruder to obtain a casting sheet, wherein the mixed oil comprises a volatile oil product and a non-volatile oil product; an oil-gas volatilization step: subjecting the cast sheet to a gas-solid separation process so that the oil and gas volatilized by the volatile oil in the mixed oil leave the cast sheet to obtain a porous membrane; as well as A post-processing step: extracting and drying the porous membrane to obtain a large pore size membrane.
2. The method according to claim 1, It is characterized in that Also includes: A mixing step: mixing the volatile oil product and the non-volatile oil product to obtain the mixed oil.
3. The method according to claim 1, It is characterized in that The gas-solid separation process includes using negative pressure to volatilize the volatile oil in the casting into the oil gas so as to leave the casting.
4. The method according to claim 1, It is characterized in that The gas-solid separation process comprises: A stretching and volatilization step: the obtained casting sheet is stretched so that the volatile oil in the casting sheet is volatilized into the oil gas and leaves the casting sheet.
5. The method according to claim 4, Features: The stretching and volatilization step further comprises the following steps: a negative pressure stretching step: stretching the casting sheet under negative pressure so that the volatile oil product evaporates from the casting sheet to form a plurality of micropores on the casting sheet; and An expansion and stretching step: the cast sheet is stretched again to further expand the micropores to form the porous membrane.
6. The method according to claim 1, It is characterized in that The post-processing steps include: an extraction step: subjecting the porous membrane to an extraction treatment to wash away the non-volatile oil product to form an extraction membrane; and A drying step: drying the extraction membrane to obtain the large-pore diaphragm.
7. The method according to claim 6, It is characterized in that Prior to the extraction step, the method further comprises the following steps: A heat preservation step: subjecting the porous membrane to heat preservation treatment.
8. The method according to claim 1, Features: It also includes the following steps: An oil and gas recovery step: recovering the oil and gas generated by volatilizing the volatile oil product in the oil and gas volatilization step.
9. The method according to claim 1, Features: The volatile oil product comprises normal, isomeric or cycloparaffin C6 mineral oil, the non-volatile oil product comprises white oil, and the plastic material comprises polyethylene.
10. The method according to claim 1, Features: The ratio between the volatile oil and the non-volatile oil is 1:(0.1-0.2).
11. The method according to claim 3, Features: In the stretching volatilization step, the negative pressure condition ranges from -500 Pa to -100 Pa relative to atmospheric pressure.
12. A large-aperture diaphragm, It is characterized in that The maximum pore size of the large-pore diaphragm is between 85 nm and 100 nm.
13. The large-pore diaphragm according to claim 12, Features: The large-pore diaphragm is prepared by the method for preparing a large-pore diaphragm by replacing an inorganic filler with a mixed oil as described in any one of claims 1 to 11.
14. The large-pore diaphragm according to claim 12, Features: The needle puncture strength of the large-pore diaphragm is greater than 80gf / μm, and the MD tensile strength of the large-pore diaphragm is greater than 800kgf / cm 2 The TD tensile strength of the large-aperture diaphragm is greater than 800 kgf / cm 2 The large-pore diaphragm has an MD elongation greater than 50% and a TD elongation greater than 50%.
15. A system for making large-aperture diaphragms by replacing inorganic fillers with mixed oil. It is characterized in that include: a mixer for mixing a volatile oil product with a non-volatile oil product to obtain a mixed oil; An extruder, used for melting and extruding the plastic material and the mixed oil to obtain a casting sheet; A protective cover, surrounding the extrusion die of the extruder, to confine the volatilization space of the volatile oil in the casting sheet within the protective cover, thereby preventing the volatile oil from diffusing and volatilizing into an open environment; a stretching and volatilization device, used for stretching the obtained cast sheet to volatilize the volatile oil product to obtain a porous membrane; An extraction device, used to perform extraction treatment on the porous membrane to wash away the non-volatile oil product to form an extraction membrane; as well as A drying device is used for drying the extraction membrane to obtain a large pore size membrane.
16. The system of claim 15, Features: The stretching volatilization device further comprises: a negative pressure stretching device, used for stretching the casting sheet under a negative pressure environment so that the volatile oil product evaporates from the casting sheet to form a plurality of micropores on the casting sheet; and An expansion and stretching device is used to stretch the cast sheet again to further expand the micropores to form the porous membrane.
17. The system of claim 15, Features: Also includes: An oil gas recovery device is used to recover the oil gas generated by the volatilization of the volatile oil product.