Anti-slip carpet with hollow net-shaped TPE (thermoplastic elastomer) film and preparation method of anti-slip carpet

By punching holes on the TPE film to form a hollow mesh structure, and combining the carrier to increase the clarity and flatness of the carpet, the existing TPE back bottom carpet has poor breathability and poor anti-slip effect, and has achieved the problem of slippery ground Efficient anti-slip and breathability improves, and improves carpet durability and production efficiency.

CN118927740APending Publication Date: 2024-11-12KUNSHAN YIJIAJU TEXTILE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411077835.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing TPE back carpet has poor breathability, is not easy to dry, is not good for slipping, and is easy to break after washing; foamed latex carpet has poor anti-aging performance, and is prone to dust during transportation, so it needs to be added. Release paper leads to additional garbage and costs; the existing anti-slip carpet with strips is not flat overall, and the suction cup-shaped breathable wet-exhaust carpet on concave and convex floors have poor anti-slip effect and low production efficiency.

Method used

Use hollow mesh TPE film as the bottom surface of the carpet, and form through holes by punching holes on the TPE film, and combine the carrier to increase clarity and flatness. Use the holes to discharge water and air to eliminate the water film effect, improve anti-slip and breathability, and pass Integrated molding structure improves durability.

Benefits of technology

It achieves good anti-slip effect on slippery ground, improves breathability and easy-to-dryness, avoids the fracture problem of strip-shaped anti-slip strips, and is suitable for flat and uneven grounds, with high production efficiency and good economicality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927740A_ABST
    Figure CN118927740A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-slip carpet with a hollow reticular TPE (thermoplastic elastomer) film and a preparation method of the anti-slip carpet. The carpet comprises a carpet body and a hollow reticular film layer which are arranged from top to bottom, a plurality of hollowed-out holes are distributed in the hollowed-out net-shaped film layer and penetrate through the hollowed-out net-shaped film layer, and the hollowed-out net-shaped film layer is integrally formed. The preparation method A comprises the following steps: A1, melting TPE, coating a carrier with the molten TPE, and forming holes to prepare a hollow reticular film layer; a2, the hollowed-out net-shaped film layer and the carpet body are bonded and compounded; the preparation method B comprises the following steps: B1, melting TPE, coating release paper with the molten TPE, and forming holes, or melting and extruding the TPE to form a film, forming holes, and compounding with the release paper to prepare a composite coiled material; b2, hot-pressing and compounding the composite coiled material and the carpet body; the preparation method C comprises the following steps: C1, melting TPE, coating the carpet body with the molten TPE, and forming holes. The prepared carpet is good in skid resistance, high in durability, good in air permeability, easy to spin-dry, good in anti-aging performance and suitable for application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile carpets and relates to an anti-slip carpet with a hollow mesh TPE film and a preparation method thereof. Background Art

[0002] With the improvement of family living environment and quality of life, more and more families are choosing to lay carpets on indoor and outdoor floors such as outside doors, living rooms, bedrooms, bathrooms, etc. Since TPE, foamed latex and acrylic resin carpet backings have certain anti-slip properties, they are increasingly used in carpet backings.

[0003] However, most TPE-backed carpets on the market currently use fully coated TPE. Since TPE is not easy to foam during coating (even if it foams, it is closed-cell foaming), fully coated TPE carpets have poor air permeability, are not easy to spin dry, and when laid on slippery surfaces, water cannot be discharged, forming a water film effect that reduces the friction coefficient and causes a deviation in the anti-slip effect. Foamed latex-backed carpets have deviated anti-aging properties due to the foamed latex's own formula and porous structure. Acrylic resin-backed carpets have strong stickiness on the back, and the carpets are particularly easy to get dusty or stick to the carpet surface during packaging or transportation. Therefore, a layer of release paper must be attached to the back of the carpet, resulting in additional waste and costs.

[0004] The existing Chinese patent with publication number CN113907588A discloses a carpet anti-skid mat with strip-shaped anti-skid strips and a method of using the same. The carpet anti-skid mat with strip-shaped anti-skid strips comprises a non-woven fabric layer and an anti-skid strip. The lower side of the non-woven fabric layer is fixed with an anti-skid strip, and the length of the anti-skid strip is the same as that of the carpet anti-skid mat. The upper surface of the non-woven fabric layer is used to place the carpet. The carpet anti-skid mat with strip-shaped anti-skid strips in this patent adopts the strip-shaped anti-skid strips as the backing, which to a certain extent solves the problems of poor air permeability, difficulty in drying, and deviation in anti-skid effect when encountering water. However, due to the structure of the strip-shaped anti-skid strips themselves, there are problems that the strip-shaped anti-skid strips are easily broken after friction after washing, and for relatively thin carpets, the carpet surface is sunken due to the overall unevenness.

[0005] In addition, the prior art also provides a carpet with a suction cup-shaped structure and a suction cup-shaped breathable and dehumidifying hole at the bottom. Through the design of the suction cup-shaped structure and the suction cup-shaped dehumidifying hole, the air in the suction cup-shaped structure is discharged from the suction cup-shaped dehumidifying hole next to it under the action of external force, thereby forming a negative pressure inside the suction cup-shaped structure, thereby making the carpet have a certain anti-slip performance. However, since multiple suction cup-shaped structures and suction cup-shaped dehumidifying holes are arranged at the bottom of the carpet, the carpet is not flat as a whole; in addition, the suction cup-shaped dehumidifying holes of the carpet are not arranged through, and the water discharge effect is too poor. It only plays an anti-slip role with the help of negative pressure, so it can only be applied to smooth and flat ground; in addition, the suction cup-shaped structure and suction cup-shaped dehumidifying holes at the bottom of the carpet are realized by injection molding a single piece of carpet, which has low production efficiency and poor economic performance. Summary of the invention

[0006] The purpose of the present invention is to provide a non-slip carpet with a hollow mesh TPE film and a preparation method thereof in view of the deficiencies of the prior art. The present invention prepares a TPE film, and then processes the TPE film to make the TPE film into a mesh TPE film with a plurality of hollow holes distributed thereon. Since the hollow holes penetrate the TPE film, when the hollow mesh TPE film contacts the slippery ground, under the action of its own gravity and external force, water and air are discharged through the holes, eliminating the water film effect, and the back of the carpet is in close contact with the ground. At the same time, the carpet surface layer located in the hole-shaped part is adsorbed with the ground, which greatly improves the anti-slip property; in addition, the hollow mesh TPE film is integrally formed, and the TPE layer of the carpet is not easy to break after multiple uses and washing, and the safety and use experience are better. The carpet prepared by the present invention has good anti-slip property, strong durability, good air permeability, easy drying, and good anti-aging performance.

[0007] The purpose of the present invention can be achieved by the following scheme:

[0008] In a first aspect, the present invention provides an anti-slip carpet with a hollow mesh TPE film, comprising a carpet body and a hollow mesh film layer arranged from top to bottom; a plurality of hollow holes are distributed on the hollow mesh film layer, and the holes penetrate the hollow mesh film layer.

[0009] As an embodiment of the present invention, the area of ​​the hole is 0.0314-400mm 2 , the spacing between adjacent holes is 0.5-200mm.

[0010] Furthermore, the area of ​​the hole is 0.1256-100mm 2, the spacing between adjacent holes is 1-7.9mm. If the hole area is too large or too small, the effect of the carpet surface layer at the hole-shaped part adsorbing the ground will be weakened, which will lead to a weakened anti-slip performance and increase the difficulty of manufacturing; if the hole area is too small, the water and air discharge effect will be too poor, which will lead to a weakened anti-slip performance. If the spacing between two adjacent holes is too large or too small, it will increase the difficulty of manufacturing; if the spacing between two adjacent holes is too large, the water and air discharge effect will be too poor, which will lead to a weakened anti-slip performance.

[0011] As an embodiment of the present invention, the hollow mesh film layer is integrally formed. Each hole of the present invention extends from the bottom surface of the hollow mesh film layer to the junction of the carpet body and the hollow mesh film layer, that is, penetrates the hollow mesh film layer.

[0012] As an embodiment of the present invention, the material of the hollow mesh membrane layer includes TPE.

[0013] Furthermore, the specific gravity of the TPE is not greater than 1.3, the Shore hardness of the TPE is 10-50A, and the content of SEBS or SBS in the TPE is 10-50wt.%. If the specific gravity of the TPE is too large, the Shore hardness is too high, and the content of SEBS or SBS in the TPE is too low, the TPE will have poor anti-slip properties; if the content of SEBS or SBS in the TPE is too high, the cost of the TPE will be too high.

[0014] As an embodiment of the present invention, the thickness of the hollow mesh film layer is 0.1-5 mm; the unit area mass of the hollow mesh film layer is 30-1500 g / m 2 .

[0015] As an embodiment of the present invention, the shape of the hole includes at least one of a circle, an ellipse, a diamond, a cross, a triangle, a rectangle, a plum blossom, a cloud, and other irregular shapes.

[0016] As an embodiment of the present invention, the carpet body includes at least one of tufted fabric, knitted fabric, woven fabric, needle-punched fabric, flocked fabric, hand-woven fabric, and non-woven fabric.

[0017] As an embodiment of the present invention, a carrier is arranged between the carpet body and the hollow mesh membrane layer.

[0018] Furthermore, the carrier includes at least one of non-woven fabric, woven fabric and knitted fabric.

[0019] According to the preparation method of the hollow mesh film layer, a carrier is arranged between the carpet body and the hollow mesh film layer, and the carrier is used to carry the hollow mesh film and increase the overall stiffness and flatness of the carpet.

[0020] In a second aspect, the present invention provides a method for preparing a non-slip carpet with a hollow mesh TPE film, the preparation method comprising any one of A, B, and C;

[0021] Preparation method A comprises the following steps:

[0022] A1, coating the melted TPE on a carrier and making holes therein to form a hollow mesh film layer with a carrier;

[0023] A2, bonding and laminating the hollow mesh film layer prepared in A1 with the carpet body to obtain the anti-slip carpet;

[0024] Preparation method B comprises the following steps:

[0025] B1. Melt TPE and apply it on the release paper and make holes.

[0026] Or, melt TPE and extrude it into a film, then make holes and laminate it with release paper.

[0027] A composite roll of a hollow mesh film layer and a release paper is produced;

[0028] B2, hot-pressing the composite coil prepared in B1 and the carpet body, separating the release paper, and obtaining the anti-slip carpet;

[0029] Preparation method C comprises the following steps:

[0030] C1. Melting TPE is applied to a carpet body and holes are made to obtain the anti-slip carpet.

[0031] As an embodiment of the present invention, in step A1 or B1 or C1, the melting method includes one of a casting machine, a coating machine, and a laminating machine.

[0032] Furthermore, the working temperature of the casting machine is 150-220°C, and the speed is 2-10 m / min; the working temperature of the coating machine is 150-220°C, and the speed is 0.5-8 m / min; the working temperature of the laminating machine is 130-250°C, and the speed is 1-10 m / min.

[0033] As an embodiment of the present invention, in step A1 or B1 or C1, the hole making method includes one of mechanical punching, laser punching, ultrasonic punching, microwave punching, and roller punching.

[0034] Furthermore, the roller punching is to pour the molten TPE through a die head onto a roller with a predetermined hole shape for punching; the surface of the roller includes a flat area and a recessed area, and the shape of the flat area is a hole shape.

[0035] The present invention uses a casting machine, a coating machine or a laminating machine to heat TPE to a molten state, and the molten TPE is poured onto a roller with a predetermined hole shape through a die head (the roller surface includes a flat area and a recessed area, and the shape of the flat area is the hole shape). At the same time, a carrier or a release paper is wound onto the roller from the bottom of the roller, and under the action of a scraper at the rear, the carrier or the release paper is tightly attached to the roller, and then under the extrusion of a pressure roller at the rear, the carrier or the release paper and the TPE are pressed together.

[0036] As an embodiment of the present invention, in step A2, the glue used for the bonding and compounding includes one of hot melt glue, TPE, styrene-butadiene rubber, water-based glue, and solvent-based glue.

[0037] In step B1 of the present invention, the specific process of melt-extruding TPE into a film, making holes, and (physically) compounding it with release paper includes: using a casting machine, a coater or a laminating machine to heat TPE to a molten state, the molten TPE passes through the die head to form a uniform film, the TPE film is quickly cooled by a cooling roller to fix the shape and structure of the film, after the film is cooled, the TPE film is punched according to a predetermined hole shape and spacing by a punching device, and then a clean release paper roll is prepared, and the punched TPE film is physically compounded with the release paper roll.

[0038] As an embodiment of the present invention, in step B2, the specific process of the hot pressing compound includes:

[0039] Place the carpet body with the bottom surface facing upward on the Teflon mesh belt, and wind the composite coil made of B1 with the hollow mesh film layer facing upward on the heating roller. As the mesh belt is conveyed forward and the heating roller is rolled, the mesh belt and the heating roller are squeezed against each other, so that the bottom surface of the carpet body is bonded to the hollow mesh film layer, and the release paper is separated accordingly.

[0040] Alternatively, the composite coil made of B1 is rolled up onto a lower pressing roller with the hollow mesh film layer facing downward, and the carpet body is rolled up onto an upper pressing roller with the bottom surface facing upward, wherein the lower pressing roller is a heating roller and the upper pressing roller is a cooling roller, and pressure is applied to bond the upper and lower layers together, and the release paper is separated.

[0041] Furthermore, the heating temperature of the heating roller is 130-230° C., the pressing pressure is 3-8 kg, and the speed is 3-9 m / min.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1. The present invention sets a hollow mesh film layer on the bottom surface of the carpet, and the hollow mesh film layer is distributed with hollow holes that penetrate the layer. When the hollow mesh TPE film contacts the slippery ground, water and air are discharged through the holes under the action of its own gravity and external force, eliminating the water film effect. The carpet back is in close contact with the ground, and the carpet surface layer located in the hole-shaped part is adsorbed with the ground, which greatly improves the anti-slip property. Compared with the carpet with a suction cup structure back at the bottom, the carpet of the present invention can also achieve a better anti-slip effect on uneven ground; in addition, the present invention can also use a lower weight TPE back as needed, saving costs while avoiding the problem of the carpet being too heavy. In addition, the present invention has high production efficiency and good economy.

[0044] 2. The present invention arranges a hollow mesh film layer on the bottom surface of the carpet, and the hollow mesh film layer is distributed with hollow holes, so that the anti-slip carpet with a porous film has excellent air permeability and is easy to dry compared to the fully coated back TPE carpet on the market, and has a better anti-slip effect after laying water on smooth and flat tiles or uneven ground.

[0045] 3. The present invention provides an integrally formed hollow mesh film layer on the bottom surface of the carpet. Compared with the strip-shaped anti-skid strips, the hollow mesh film layer is not easy to break after washing, and the water washing performance is close to that of a fully coated TPE. For relatively thin carpets, the strip-shaped anti-skid strips will not cause the overall unevenness of the carpet and cause the carpet surface to sag. Compared with foamed latex backed carpets, the anti-aging performance is better.

[0046] 4. The present invention can also use a hollow mesh film layer with a carrier, which is beneficial to increase the overall stiffness and flatness of the carpet. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0048] Figure 1 Schematic diagram of the cross-sectional structure of the carpet in Examples 1, 2, and 5;

[0049] Figure 2 Schematic diagram of the cross-sectional structure of the carpet in Examples 3, 4, and 6;

[0050] Figure 3 It is a schematic diagram of the cross-sectional structure of a hollow mesh membrane layer in an embodiment of the present invention;

[0051] Figure 4 This is a bottom view of the hollow mesh membrane layer of Example 3 of the present invention;

[0052] Figure 5 It is a bottom view of the hollow mesh membrane layer of Example 4 of the present invention;

[0053] Figure 6 This is a bottom view of the hollow mesh membrane layer of Example 5 of the present invention;

[0054] Figure 7 This is a bottom view of the hollow mesh membrane layer of Example 1 of the present invention;

[0055] Figure 8 This is a bottom view of the hollow mesh membrane layer of Example 2 of the present invention;

[0056] Figure numerals: 1, carpet body; 2, hollow mesh membrane layer; 3, holes; 4, carrier. DETAILED DESCRIPTION

[0057] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.

[0058] Example 1

[0059] This embodiment provides a method for preparing a non-slip carpet with a hollow mesh TPE film, the carpet structure is as follows Figure 1 As shown, the preparation steps are as follows:

[0060] Step 1: Use a casting machine to heat the TPE particles to a molten state. The molten TPE passes through the casting machine head to form a uniform film. The TPE film is quickly cooled by a cooling roller to fix the shape and structure of the film. After the film is cooled, a mechanical punching device is used to punch holes 3 in the TPE film according to the shape and spacing of the predetermined holes. Then a clean release paper roll is prepared, and the punched TPE film is physically compounded with the release paper roll to form a composite roll of a hollow mesh film layer 2 and a release paper. The shape of the hole 3 is a diamond, and the area of ​​the hole 3 is 8.66mm 2 , the spacing between adjacent holes 3 is 30mm, the working temperature of the casting machine is 200℃, the speed is 5m / min; the TPE model is TPE_KBT-15A-1, the SEBS content is 40%, the color is colorless and transparent, the HS hardness is 15A, the specific gravity is 0.9, and the usage is 200g / m 2 , thickness is 0.5mm.

[0061] Step 2: Select a polyester flat woven blanket with a square gram weight of 1100gsm, that is, the carpet body 1. Wind the hollow mesh film layer 2 of the composite coil made in step 1 onto the lower pressure roller with the surface facing downward, and wind the carpet body 1 onto the upper pressure roller with the bottom surface facing upward, wherein the lower pressure roller is a heating roller and the upper pressure roller is a cooling roller, and apply pressure to make the upper and lower layers bond together, and the release paper is separated. The temperature of the heating roller is 190°C and the pressure is 5 kg. The cross-sectional structure and the bottom view of the hollow mesh film layer 2 are shown in Figure 2 and Figure 2 respectively. Figure 3 , Figure 7 shown.

[0062] Step 3: Cut the blank carpet obtained in step 2 to a size of 50X80 cm, and use 40s / 3 polyester sewing thread for hemming with a hemming width of 10 mm to obtain the anti-slip carpet with a hollow mesh TPE film of the present invention.

[0063] Example 2

[0064] This embodiment provides a method for preparing a non-slip carpet with a hollow mesh TPE film, the carpet structure is as follows Figure 1 As shown, the preparation steps are as follows:

[0065] Step 1: Select a polyester cut pile tufted carpet with a pile height of 35mm and a base fabric of 100gsm PP woven base fabric, that is, the carpet body 1, and the weight of the carpet is 860gsm. Use a TPE laminating machine to melt TPE and apply it to the bottom surface of the carpet body 1, and then laser punch the composite carpet according to the shape and spacing of the predetermined holes 3 to obtain a carpet with a hollow mesh film layer 2 on the bottom. The shape of the hole 3 is a cross, and the area of ​​the hole 3 is 36mm 2 The spacing between the three holes is 50mm. The laminating machine has an operating temperature of 210℃ and a speed of 4m / min. The TPE model is TPE_KBT-50A-1, the SEBS content is 21%, the color is dark gray, the HS hardness is 50A, the specific gravity is 1.3, and the usage is 500g / m 2 , with a thickness of 0.8 mm. The laser power of the laser drilling device is 80 W, the pulse width is 15 nanoseconds, and the pulse frequency is 20 kHz. The cross-sectional structure and bottom view of the hollow mesh film layer 2 are shown in FIG. Figure 3 , Figure 8 shown.

[0066] Step 2: Cut the blank carpet obtained in step 1 into a size of 50x80 cm, use 2020D polyester D3-2 edge-locking yarn for edge-locking, and the edge-locking width is 7 mm to obtain the anti-slip carpet with a hollow mesh TPE film of the present invention.

[0067] Example 3

[0068] This embodiment provides a method for preparing a non-slip carpet with a hollow mesh TPE film. The carpet structure is as follows: Figure 2 As shown, the preparation steps are as follows:

[0069] Step 1: Select a square weight of 350g / m 2 A roll of polyester nonwoven fabric is prepared, TPE is melted by a TPE laminating machine and coated on the polyester nonwoven fabric, and then mechanical punching is used to pass the composite fabric through a rotating hot pricking roller with raised thorns of predetermined hole 3 shape and spacing on the top, so as to obtain a hollow mesh film layer 2 with polyester nonwoven fabric (i.e., carrier 4). The shape of hole 3 is circular, and the area of ​​hole 3 is 28.26mm 2 The spacing between the three holes is 6mm. The laminating machine has an operating temperature of 210℃ and a speed of 5m / min. The TPE model is TPE_KBT-001N, the SEBS content is 28%, the color is white, the Shore hardness is 30A, the specific gravity is 1.19, and the usage is 350g / m 2 The thickness is 0.6 mm; the heating temperature of the hot piercing roller is 90°C and the speed is 5 m / min. The cross-sectional structure and bottom view of the hollow mesh film layer 2 are shown in FIG. Figure 3 , Figure 4 shown.

[0070] Step 2: Select a square weight of 350g / m 2 The polyester knitted blank blanket, that is, the carpet body 1, is passed through a composite machine with 15g / m 2 The PUR hot melt adhesive is compounded with the hollow mesh membrane layer 2 with polyester non-woven fabric obtained in step 1, and the bottom surface of the carpet body 1 is connected to the surface of the hollow mesh membrane layer 2 where the polyester non-woven fabric is located, so as to obtain a compounded blank carpet.

[0071] Step 3: Cut the blank carpet obtained in step 2 to a size of 50x80 cm, use 2020D polyester D3-2 edge-locking yarn for edge-locking, and the edge-locking width is 7 mm to obtain the anti-slip carpet with a hollow mesh TPE film of the present invention.

[0072] Example 4

[0073] This embodiment provides a method for preparing a non-slip carpet with a hollow mesh TPE film, the carpet structure is as follows Figure 2 As shown, the preparation steps are as follows:

[0074] Step 1: Select a square weight of 100g / m 2A roll of polyester non-woven fabric. The TPE is heated to a molten state using a coating machine. The molten TPE is poured through a die head onto a roller with a predetermined hole 3 shape and spacing. At the same time, the polyester non-woven fabric is wound onto the roller from the bottom of the roller. Under the action of the scraper at the rear, the polyester non-woven fabric is tightly attached to the roller. Then, under the extrusion of the pressure roller at the rear, the polyester non-woven fabric and TPE are pressed together to form a hollow mesh membrane layer 2 with polyester non-woven fabric. The shape of the hole 3 is elliptical, and the area of ​​the hole 3 is 17.52mm 2 , the spacing between the three holes is 20mm, the working temperature of the coating machine is 200℃, the speed is 4m / min; the TPE model is TPE_KBT-C002, the SEBS content is 23%, the color is camel, the HS hardness is 45A, the specific gravity is 1.26, and the usage is 400g / m 2 , with a thickness of 0.6 mm. The cross-sectional structure and bottom view of the hollow mesh film layer 2 are shown in FIG. Figure 3 , Figure 5 shown.

[0075] Step 2: Select a pile height of 18mm and a base fabric of 100g / m 2 Polyester cut pile tufted blanket with PP woven base fabric is used as a standby, that is, the carpet body 1, and the blanket weight is 720g / m 2 The carpet body 1 is laminated with the hollow mesh film layer 2 with polyester non-woven fabric obtained in step 1 by TPE laminating machine, and the bottom surface of the carpet body 1 is connected with the polyester non-woven fabric surface of the hollow mesh film layer 2 to obtain a laminated blank carpet. The laminating machine has an operating temperature of 195°C and a speed of 5 m / min; the TPE model is TPE_KBT-40A-1, the SEBS content is 15%, the color is white, the Shore hardness (HShardness) is 40A, the specific gravity is 1.25, and the usage is 400g / m 2 .

[0076] Step 3: Cut the blank carpet obtained in step 2 to a size of 50x80 cm, use 2020D polyester D3-2 edge-locking yarn for edge-locking, and the edge-locking width is 7 mm to obtain the anti-slip carpet with a hollow mesh TPE film of the present invention.

[0077] Example 5

[0078] This embodiment provides a method for preparing a non-slip carpet with a hollow mesh TPE film, the carpet structure is as follows Figure 2 As shown, the preparation steps are as follows:

[0079] Step 1: Use a coating machine to heat TPE to a molten state. The molten TPE is poured through the die head onto a roller with a predetermined hole 3 shape and spacing. At the same time, the release paper is wound onto the roller from the bottom of the roller. Under the action of the scraper at the rear, the release paper is tightly attached to the roller. Then, under the extrusion of the pressure roller at the rear, the release paper and TPE are pressed together to form a composite roll of the hollow mesh film layer 2 and the release paper. The shape of the hole 3 is plum blossom, and the area of ​​the hole 3 is 125.5mm 2 The spacing between the three holes is 200mm, the coating machine operating temperature is 200℃, the speed is 4.5m / min; the TPE model is TPE_KBT-15A-1, the SEBS content is 40%, the color is colorless and transparent, the HS hardness is 15A, the specific gravity is 0.9, and the usage is 180g / m 2 , with a thickness of 0.4 mm. The cross-sectional structure and bottom view of the hollow mesh film layer 2 are shown in FIG. Figure 3 , Figure 6 shown.

[0080] Step 2: Select a polyester cut pile tufted blanket with a pile height of 26mm and a base fabric of 100gsm PP woven base fabric, that is, the carpet body 1, and the blanket weight is 1050gsm. Place the carpet body with the bottom surface facing up on the Teflon mesh belt, and wind the hollow mesh film layer 2 of the composite coil prepared in step 1 onto the heating roller with the surface facing up. As the mesh belt is conveyed forward and the heating roller is rolled, the mesh belt and the heating roller are squeezed mutually, so that the bottom surface of the carpet body is bonded to the hollow mesh film layer 2, and the release paper is separated. The temperature of the heating roller is 190℃ and the pressure is 5 kg.

[0081] Step 3: Cut the blank carpet obtained in step 2 to a size of 50x80 cm, use 2020D polyester D3-2 edge-locking yarn for edge-locking, and the edge-locking width is 7 mm to obtain the anti-slip carpet with a hollow mesh TPE film of the present invention.

[0082] Example 6

[0083] The preparation method of this embodiment is basically the same as that of embodiment 3, except that the amount of TPE used in step 1 is 1500 g / m 2 .

[0084] Comparative Example 1

[0085] The preparation method of this comparative example is basically the same as that of Example 3, except that the hollow mesh film layer 2 is not prepared, but the conventional full-coating TPE method is used for the backing.

[0086] The preparation steps are as follows:

[0087] Step 1: Select a square weight of 350g / m2 The polyester knitted blanket, that is, the carpet body 1; the square gram weight is 350g / m 2 The carpet body 1 is passed through a composite machine using 15g / m 2 The PUR hot melt adhesive is compounded with the polyester non-woven fabric, and the bottom surface of the carpet body 1 is connected with the top surface of the polyester non-woven fabric to obtain a compounded green carpet.

[0088] Step 2: Use a TPE laminating machine to melt-coat the TPE on the bottom surface of the composite blanket obtained in step 1. The die head used by the laminating machine is a full-coating TPE die head; the laminating machine has an operating temperature of 210°C and a speed of 5 m / min; the TPE model is TPE_KBT-001N, the SEBS content is 28%, the color is white, the Shore hardness (HS hardness) is 30A, the specific gravity is 1.19, and the usage is 350g / m 2 .

[0089] Step 3: Cut the blank carpet obtained in step 2 into a size of 50x80cm, use 2020D polyester D3-2 edge yarn for edge locking, and the edge locking width is 7mm to obtain a carpet.

[0090] Comparative Example 2

[0091] The preparation method of this comparative example is basically the same as that of Example 3, except that a strip TPE method is used for backing instead of preparing a hollow mesh film layer 2 .

[0092] The preparation steps are as follows:

[0093] Step 1: Select a square weight of 350g / m 2 The polyester knitted blanket, that is, the carpet body 1; the square gram weight is 350g / m 2 The carpet body 1 is passed through a composite machine using 15g / m 2 The PUR hot melt adhesive is compounded with the polyester non-woven fabric, and the bottom surface of the carpet body 1 is connected with the top surface of the polyester non-woven fabric to obtain a compounded green carpet.

[0094] Step 2: Use a TPE laminating machine to melt-coat the TPE on the bottom surface of the composite blanket obtained in step 1. The die used by the laminating machine is a strip TPE die, the strip TPE width is 10mm, the spacing is 10mm; the laminating machine has an operating temperature of 210℃ and a speed of 5 meters / minute; the TPE model is TPE_KBT-001N, the SEBS content is 28%, the color is white, the Shore hardness (HShardness) is 30A, the specific gravity is 1.19, and the usage is 350g / m 2 .

[0095] Step 3: Cut the blank carpet obtained in step 2 into a size of 50x80cm, use 2020D polyester D3-2 edge-locking yarn for edge-locking, and the edge-locking width is 7mm to obtain a carpet.

[0096] Comparative Example 3

[0097] The preparation method of this comparative example is compared with that of Example 3. The carpet body and the polyester non-woven fabric are exactly the same, and the difference is that the backing is made of foamed latex.

[0098] The preparation steps are as follows:

[0099] Step 1: Select a square weight of 350g / m 2 The polyester knitted blanket, that is, the carpet body 1; the square gram weight is 350g / m 2 The carpet body 1 is passed through a composite machine using 15g / m 2 The PUR hot melt adhesive is compounded with the polyester non-woven fabric, and the bottom surface of the carpet body 1 is connected with the top surface of the polyester non-woven fabric to obtain a compounded green carpet.

[0100] Step 2: Use light grey foam latex to back glue the blank blanket obtained in step 1, with a foaming ratio of 550 g / L, a temperature of 140° C., and a glue amount of 600 gsm.

[0101] Step 3: Cut the blank carpet obtained in step 2 into a size of 50x80cm, use 2020D polyester D3-2 edge yarn for edge locking, and the edge locking width is 7mm to obtain a carpet.

[0102] Comparative Example 4

[0103] The preparation method of this comparative example is different from that of Example 3 in that the area of ​​hole 3 is 0.0314 mm 2 The spacing between two adjacent holes 3 is 0.5 mm.

[0104] Comparative Example 5

[0105] The preparation method of this comparative example is different from that of Example 3 in that the area of ​​hole 3 is 314 mm 2 The distance between two adjacent holes is 120mm.

[0106] Comparative Example 6

[0107] The preparation method of this comparative example is different from that of Example 3 only in that the TPE model is TPE_KBT-70A-1, the SEBS content is 14%, the color is white, the Shore hardness (HS hardness) is 70A, and the specific gravity is 1.37.

[0108] Comparative Example 7

[0109] The preparation method of this comparative example is different from that of Example 6 in that the structure of the hole 3 is replaced by a suction cup-shaped breathable and moisture-desorption hole.

[0110] The preparation steps are as follows:

[0111] Step 1: Select a square weight of 350g / m 2 Polyester nonwoven fabric with a square gram weight of 350g / m 2 One roll of polyester knitted blanket is passed through a composite machine with 15g / m 2 The bottom surface of the polyester knitted blanket is connected with the top surface of the polyester non-woven fabric by compounding them with PUR hot melt adhesive.

[0112] Step 2: Cut the composite blanket obtained in step 1 into a size of 51 x 81 cm.

[0113] Step 3: Place the 51x81cm blanket obtained in step 2 into the mold. There are four symmetrical upper and lower fixed pillars around the mold to fix it. The middle of the mold is hollowed out into a suction cup-shaped breathable and moisture-desorption hole. Specifically, the bottom is suction cup-shaped and the top is cylindrical, which are integrated with each other. Use an injection molding machine to melt TPE_KBT-001N, with a SEBS content of 28%, white color, Shore hardness (HS hardness) of 30A, and a specific gravity of 1.19 at a high temperature of 200°C and inject it from the left side of the mold. The TPE molten liquid fills the mold in 10 seconds and is pressed up and down. After cooling, the blanket and TPE form a whole, the mold is opened, and it is taken out. The suction cup-shaped part of the suction cup-shaped breathable and moisture-desorption hole is a circle with a diameter of 6mm, and the corresponding area is 28.26mm 2 The cylindrical part of the suction cup-shaped breathable and dehumidifying hole is a circle with a diameter of 1 mm, and the distance between two adjacent suction cup-shaped breathable and dehumidifying holes is 6 mm.

[0114] Step 4: Trim the carpet obtained in step 3 to a size of 50x80cm after trimming. Use 2020D polyester D3-2 lock-edge yarn for lock-edge, with a lock-edge width of 7mm to obtain a carpet with suction cup-shaped breathable and moisture-desorption holes.

[0115] Comparative Example 8

[0116] The preparation method of this comparative example is different from that of Example 6 in that the structure of the hole 3 is replaced by a suction cup-shaped structure and a suction cup-shaped breathable and moisture-desorption hole.

[0117] The preparation steps are as follows:

[0118] Step 1: Select a square weight of 350g / m 2 Polyester nonwoven fabric with a square gram weight of 350g / m 2One roll of polyester knitted blanket is passed through a composite machine with 15g / m 2 The bottom surface of the polyester knitted blanket is connected with the top surface of the polyester non-woven fabric by compounding them with PUR hot melt adhesive.

[0119] Step 2: Cut the composite blanket obtained in step 1 into a size of 51 x 81 cm.

[0120] Step 3: Place the 51x81cm blanket obtained in step 2 into the mold. There are four symmetrical fixed pillars around the mold to fix it. The middle of the mold is hollowed out to form a suction cup-shaped structure and a suction cup-shaped breathable and moisture-desorption hole. The suction cup-shaped breathable and moisture-desorption hole is specifically a suction cup-shaped hole at the bottom and a cylindrical hole at the top, which are integrated with each other. Use an injection molding machine to melt TPE_KBT-001N, with a SEBS content of 28%, white color, a Shore hardness (HS hardness) of 30A, and a specific gravity of 1.19 at a high temperature of 200°C and inject it from the left side of the mold. The TPE molten liquid fills the mold in 10 seconds and is pressed up and down. After cooling, the blanket and TPE form a whole, the mold is opened, and it is taken out. The suction cup-shaped structure is a circle with a diameter of 6mm, corresponding to an area of ​​28.26mm 2 The suction cup-shaped part of the suction cup-shaped breathable and moisture-removing hole is a circle with a diameter of 6 mm, and the corresponding area is 28.26 mm 2 The cylindrical part of the suction cup-shaped breathable and dehumidifying hole is a circle with a diameter of 1 mm. The suction cup-shaped structure and the suction cup-shaped breathable and dehumidifying hole are arranged at intervals, and the interval between them is 6 mm.

[0121] Step 4: Trim the carpet obtained in step 3 to a size of 50x80cm after trimming. Use 2020D polyester D3-2 edge yarn for edge locking with an edge locking width of 7mm to obtain a carpet with a suction cup-like structure and suction cup-like breathable and moisture-dissipating holes.

[0122] Performance Testing

[0123] 1. Anti-slip comparison test

[0124] Test method: select the anti-skid carpet with hollow mesh TPE film in Example 3 of the present invention, the carpet with conventional full TPE backing in Comparative Example 1, the carpet with too small hole area and spacing in Comparative Example 4, the carpet with too large hole area and spacing in Comparative Example 5, the carpet with too high TPE Shore hardness (HS hardness) in Comparative Example 6, the anti-skid carpet with high TPE backing weight and hollow mesh TPE film in Example 6, the carpet with suction cup-shaped breathable and dehumidification holes in Comparative Example 7, and the carpet with suction cup-shaped structure and suction cup-shaped breathable and dehumidification holes in Comparative Example 8, a 100X100cm tile, a steel ruler, a pressing plate with a size of 50x50cm and a mass of 135g, a weight with a mass of 2500g, a 500ml beaker, and some tap water for use, and use a portable tensile scale with model HL-139 to test the anti-skid values ​​of the test samples pulled the same distance on the contact surface.

[0125] The specific steps are as follows:

[0126] (1) Sampling

[0127] <1. Select one anti-slip carpet in Example 3 of the present invention, the square gram weight of the carpet is 1065g / m 2 , cut into 50X60cm sizes and numbered A1, A2, A3, A4;

[0128] <2. Select one anti-slip carpet in Comparative Example 1 of the present invention, the square gram weight of the carpet is 1065g / m 2 , cut into 50X60cm size, numbered B1, B2, B3, B4;

[0129] <3. Select one anti-slip carpet in Comparative Example 4 of the present invention, the square gram weight of the carpet is 1065g / m 2 , cut into 50X60cm size and numbered as C1, C2, C3, C4;

[0130] <4. Select one anti-slip carpet in comparative example 5 of the present invention, the square gram weight of the carpet is 1065g / m 2 , cut into 50X60cm size, numbered D1, D2, D3, D4;

[0131] <5. Select one anti-slip carpet in Comparative Example 6 of the present invention, the square gram weight of the carpet is 1065g / m 2 , cut into 50X60cm size, numbered E1, E2, E3, E4;

[0132] <6. Select one anti-slip carpet in Example 6 of the present invention, the square gram weight of the carpet is 2215g / m 2, cut into 50X60cm size and numbered F1, F2, F3, F4;

[0133] <7. Select one anti-slip carpet in Comparative Example 7 of the present invention, the square gram weight of the carpet is 2215g / m 2 , cut into 50X60cm size, numbered G1, G2, G3, G4;

[0134] <8. Select one anti-slip carpet in Comparative Example 8 of the present invention, the square gram weight of the carpet is 2215g / m 2 , cut into 50X60cm size and numbered H1, H2, H3, and H4 respectively.

[0135] (2) Testing

[0136] <1. Anti-slip test on smooth and flat tiles without water:

[0137] Place the test sample flat on a smooth ceramic tile, place a 50x50cm pressure plate with a mass of 135g on the carpet body of the test sample, align it with the three sides of the test sample, leave 50X10cm of the carpet body, place a 2500g weight in the center of the pressure plate, and use a portable tensile scale model HL-139 to test the maximum tensile force value of the test sample when it is pulled 10cm on the tile. Use this method to test test samples A1, B1, C1, D1, E1, F1, G1, and H1 respectively;

[0138] <2. Water-resistant test on smooth and flat tiles:

[0139] Use a measuring cup to take 200ml of tap water and pour it on a smooth tile. Then place the test sample flat on the tile with water. Place a 50x50cm pressure plate with a mass of 135g on the carpet body of the test sample, align it with the three sides of the test sample, leave 50X10cm of the carpet body, and place a 2500g weight in the center of the pressure plate. After an interval of 10 seconds, use a portable tensile scale with model HL-139 to test the maximum tensile force value of the test sample when it is pulled 10cm on the tile. Use this method to test test samples A2, B2, C2, D2, E2, F2, G2, and H2 respectively;

[0140] <3. Anti-slip test on uneven ground without water:

[0141] Place the test sample flat on the uneven ground, place a 50x50cm pressure plate with a mass of 135g on the carpet body of the test sample, align it with the three sides of the test sample, leave 50X10cm of the carpet body, place a 2500g weight in the center of the pressure plate, and use a portable tension scale with model HL-139 to test the maximum tension value of the test sample when it is pulled 10cm on the ground. Use this method to test test samples A3, B3, C3, D3, E3, F3, G3, and H3 respectively;

[0142] <4. Anti-slip test of laying water on uneven ground:

[0143] Use a measuring cup to take 200ml of tap water and pour it on the uneven ground. Then place the test sample flat on the ground with water. Place a 50x50cm pressure plate with a mass of 135g on the carpet body of the test sample, align it with the three sides of the test sample, leave 50X10cm of the carpet body, and place a 2500g weight at the center of the pressure plate. After an interval of 10 seconds, use a portable tension scale with model HL-139 to test the maximum tension value of the test sample when it is pulled 10cm on the ground. Test samples A4, B4, C4, D4, E4, F4, G4, and H4 respectively in this way.

[0144] The following is the test data:

[0145]

[0146] In summary, compared with Example 3, the conventional carpet fully coated with TPE backing in Comparative Example 1 has a poor anti-skid effect when laying water on smooth and flat tiles; the hole area and spacing of the carpets in Comparative Examples 4 and 5 are too small or too large, which weakens the effect of the carpet surface layer located in the hole-shaped part to adsorb the ground, and causes the water and air discharge effect to be too poor, thereby reducing its anti-skid performance, especially the anti-skid effect when laying water on smooth and flat tiles; the TPE Shore hardness (HShardness) used in the carpet in Comparative Example 6 is too high, resulting in poor anti-skid property of TPE, thereby reducing the anti-skid performance of the carpet.

[0147] Compared with Example 6, the carpet with suction cup-shaped breathable and dehumidifying holes in Comparative Example 7 is not suitable for anti-skid on smooth and flat tiles paved with water or on uneven ground, and its anti-skid effect is poor; the carpet with a suction cup-shaped structure and suction cup-shaped breathable and dehumidifying holes in Comparative Example 8, the suction cup structure is not sufficient to adsorb the ground under a small load, and the anti-skid performance on smooth and flat tiles paved with water or on uneven ground is poor.

[0148] 2. Washing appearance comparison test

[0149] Test method: The anti-slip carpet with a hollow mesh TPE film in Example 3 of the present invention and the carpet with a strip TPE backing in Comparative Example 2 were selected, and washed and dried for 1, 3, and 5 times respectively. Then, the appearance changes of the bottoms of the test samples were observed and rated in comparison with the original samples.

[0150] The specific test steps are as follows:

[0151] <1. Select two anti-slip carpets with hollow mesh TPE films in Example 3 of the present invention, and the square gram weight of the carpet is 1065g / m 2 , size is 50X80cm;

[0152] <2. Select two strips of TPE-backed carpets from Comparative Example 2 of the present invention, the square weight of the carpet is 1065 g / m 2 , size is 50X80cm;

[0153] <3. Put one of each test sample into the washing machine for washing at the same time. The washing temperature is 45℃, and the washing time is 35 minutes each time. The drying temperature is 70℃, and the drying time is 15 minutes each time. The washing and drying times are 1 time, 3 times, and 5 times. After different washing times, observe the changes in the bottom appearance of the test samples compared with the original samples and rate them.

[0154] The test results are as follows:

[0155] The appearance changes of the bottom of the test sample after washing and drying once:

[0156] Change in appearance of the bottom of the carpet in Example 3: 4.5;

[0157] Change in bottom appearance of the carpet in Comparative Example 2: Grade 4.5.

[0158] The appearance changes of the bottom of the test sample after washing and drying 3 times:

[0159] Change in appearance of the bottom of the carpet in Example 3: 4.5;

[0160] Change in bottom appearance of the carpet in Comparative Example 2: Grade 4.0 (minor breaks occurred in the strip-shaped TPE strips).

[0161] The appearance changes of the bottom of the test sample after washing and drying 5 times:

[0162] Change in appearance of the bottom of the carpet in Example 3: 4.5;

[0163] Change in bottom appearance of the carpet in Comparative Example 2: Grade 3.5 (strip-shaped TPE strips were slightly broken).

[0164] In summary, since the backing TPE of the anti-slip carpet with a hollow mesh TPE film in Example 3 of the present invention is an integrated structure, and the backing TPE of the strip TPE backing carpet in Comparative Example 2 is a relatively independent strip structure, the TPE layer of the carpet of the present invention is not easy to break due to friction after multiple uses and washings, and the safety and use experience are better.

[0165] 3. Anti-aging performance comparison test

[0166] Test method: The anti-slip carpet with a hollow mesh TPE film in Example 3 of the present invention and the carpet with a foamed latex backing in Comparative Example 3 were selected, and the carpets were cut into 5 test samples of 20x5 cm in a circulating air oven. Four of the test samples were placed in the oven and dried at 120°C. One test sample was taken out of the oven every 24h, 48h, 72h, and 96h, and the stickiness, color, cracking, and breakage after bending of the bottom of the test samples were observed compared with the original samples.

[0167] The specific test steps are as follows:

[0168] <1. Select a non-slip carpet with a hollow mesh TPE film in Example 3 of the present invention, the square gram weight of the carpet is 1065g / m 2 , the size is 50X80cm, cut it into 5 test samples of 20x5cm;

[0169] <2. Select a carpet with a foamed latex backing in Comparative Example 3 of the present invention, the square gram weight of the carpet is 1315g / m 2 , the size is 50X80cm, cut it into 5 test samples of 20x5cm;

[0170] <3. Heat the oven to 120°C, place 4 test samples of Example 3 and Comparative Example 3 on the grid of the oven, with the back side facing upward; take out a test sample from the oven every 24h, 48h, 72h, and 96h, cool the test sample for at least 15 minutes, and compare the test sample with the original sample, and evaluate the test sample according to the following evaluation criteria:

[0171] Stickiness: non-sticky / sticky;

[0172] Color changes: yellow, beige, brown, etc.;

[0173] Cracking: longitudinal / transverse: no cracking / slight cracking / moderate cracking / severe cracking;

[0174] Bending fracture: Longitudinal / Transverse: No cracking / Slight cracking / Moderate cracking / Severe cracking.

[0175] The test results are as follows:

[0176] The anti-aging performance test results of the anti-slip carpet with a hollow mesh TPE film in Example 3 of the present invention are as follows:

[0177]

[0178] The anti-aging performance test results of the carpet with foamed latex backing in Comparative Example 3 of the present invention are as follows:

[0179]

[0180]

[0181] In summary, since the TPE backing structure of the anti-slip carpet with a hollow mesh TPE film in Example 3 of the present invention is stable, the anti-aging performance is good; while the foamed latex backing of the carpet with a foamed latex backing in Comparative Example 3 changes color under high temperature conditions due to its own formula, porous structure and other reasons, and after being baked for 72 hours and 96 hours, slight cracks occur after bending, so the anti-aging performance is deviated. Therefore, the carpet of the present invention has better anti-aging performance.

[0182] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A non-slip carpet with a hollow mesh TPE film, characterized in that: The anti-slip carpet comprises a carpet body and a hollow mesh film layer which are arranged from top to bottom; a plurality of hollow holes are distributed on the hollow mesh film layer, and the holes penetrate the hollow mesh film layer.

2. The anti-slip carpet according to claim 1, characterized in that: The area of ​​the hole is 0.0314-400mm 2 , the spacing between adjacent holes is 0.5-200mm.

3. The anti-slip carpet according to claim 1, characterized in that: The area of ​​the hole is 0.1256-100mm 2 , the spacing between adjacent holes is 1-7.9 mm.

4. The anti-slip carpet according to claim 1, characterized in that: The material of the hollow mesh film layer includes TPE; the specific gravity of the TPE is not greater than 1.3, the Shore hardness of the TPE is 10-50A, and the content of SEBS or SBS in the TPE is 10-50wt.%.

5. The anti-slip carpet according to claim 1, characterized in that: The thickness of the hollow mesh film layer is 0.1-5 mm; the unit area mass of the hollow mesh film layer is 30-1500 g / m 2 .

6. The anti-slip carpet according to claim 1, characterized in that: The carpet body comprises at least one of tufted fabric, knitted fabric, woven fabric, needle-punched fabric, flocked fabric, hand-woven fabric and non-woven fabric.

7. The anti-slip carpet according to claim 1, characterized in that: A carrier is also arranged between the carpet body and the hollow mesh membrane layer, and the carrier includes at least one of non-woven fabric, woven fabric and knitted fabric.

8. A method for preparing the anti-slip carpet according to any one of claims 1 to 7, wherein the preparation method comprises any one of A, B, and C; Preparation method A comprises the following steps: A1, coating the melted TPE on a carrier and making holes therein to form a hollow mesh film layer with a carrier; A2, bonding and laminating the hollow mesh film layer prepared in A1 with the carpet body to obtain the anti-slip carpet; Preparation method B comprises the following steps: B1. Melt TPE and apply it on the release paper and make holes. Or, melt TPE and extrude it into a film, then make holes and laminate it with release paper. A composite roll of a hollow mesh film layer and a release paper is produced; B2, hot-pressing the composite coil prepared in B1 and the carpet body, separating the release paper, and obtaining the anti-slip carpet; Preparation method C comprises the following steps: C1. Melting TPE is applied to a carpet body and holes are made to obtain the anti-slip carpet.

9. The preparation method according to claim 8, characterized in that: In step A1 or B1 or C1, the melting method includes one of a casting machine, a coating machine, and a laminating machine; the working temperature of the casting machine is 150-220°C, and the speed is 2-10 m / min; the working temperature of the coating machine is 150-220°C, and the speed is 0.5-8 m / min; the working temperature of the laminating machine is 130-250°C, and the speed is 1-10 m / min.

10. The preparation method according to claim 8, characterized in that: In step A1 or B1 or C1, the hole making method includes one of mechanical punching, laser punching, ultrasonic punching, microwave punching, and roller punching.

Citation Information

Patent Citations

  • Moisture-absorbing loop pile polyester carpet and manufacturing method thereof

    CN111809409A

  • TPE bottom and back frame integrated carpet and preparation method thereof

    CN118000570A

  • Self-adhesive film comprising an antiskid coating layer

    CN1688666A

  • Luminous carpet

    CN210989568U

  • non-slip mat for automobile

    KR200312133Y1