PVC sports floor rubber and preparation method thereof
By adding porous fillers and nano zinc oxide to the foam layer of PVC sports flooring, the problems of uneven foaming and easy breakage are solved, and the shock absorption and mechanical properties of the foam layer are improved.
Patent Information
- Application Number
- CN202410992934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing PVC sports flooring has foam layers with inconsistent foam size and uneven foaming, which makes it prone to cracking, resulting in low strength and toughness of the foam layer.
Porous fillers and nano zinc oxide are added to the foaming layer. The porous fillers increase the specific surface area of the foaming agent and reduce the activation energy of the reaction, while the nano zinc oxide provides more active sites, ensuring uniform dispersion of bubbles and a dense structure of the foaming layer.
This process achieves uniform and dense foaming in the foam layer, improving the shock absorption and mechanical properties of PVC sports flooring, and enhancing the flexibility and wear resistance of the foam layer.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sports flooring, relates to PVC materials, and specifically relates to a PVC sports flooring and a preparation method thereof. Background Art
[0002] PVC sports flooring is a kind of flooring developed specifically for sports venues using polyvinyl chloride materials. PVC sports flooring has certain shock-absorbing properties and has a certain rebound ability to protect athletes when impacted. This relies on the foaming layer in the PVC sports flooring. The foaming layer is made by a foaming agent generating gas to expand the PVC material. The interior is filled with bubbles, making the foaming layer like a cushion with air inside, providing a cushioning effect for athletes and reducing the risk of athletes falling during exercise.
[0003] The most commonly used foaming agent at present is azodicarbonamide, also called AC foaming agent, which produces nitrogen, carbon monoxide, carbon dioxide and ammonia when decomposed by heat; however, AC foaming agent will also release a large amount of heat and gas instantly when decomposed at high temperature. The large amount of heat will cause the viscoelasticity of the PVC melt to further decrease, and the rapidly released gas will easily cause the initial bubble nucleus to be unevenly distributed and cause some bubble holes to rupture, making it impossible to control the structure and size of the bubble during the entire foaming process, which ultimately causes a significant reduction in the shock absorption performance of the product.
[0004] Chinese patent publication number CN110628147A discloses a modified PVC foam floor mat and a preparation method thereof. Ultrafine metal powder is added to the foam layer to reduce the pore size of the composite material and improve the uniformity of pore distribution. However, it is affected by the dispersibility of the ultrafine metal powder in the PVC foam layer, and the ultrafine metal powder may agglomerate with other fillers, resulting in uneven foaming of the foam layer. Summary of the invention
[0005] The purpose of the present invention is to provide a PVC sports flooring and a preparation method thereof, so as to solve the problems that the foaming layer has different sizes of foams, the foaming is uneven, and the foams are easy to rupture during foaming, resulting in low strength and toughness of the foaming layer.
[0006] The invention increases the specific surface area of the filler by adding porous fillers into the foaming layer, so that the foam bodies generated by the foaming agent are more uniform and denser, and reduces the reaction activation energy of the foaming agent by compounding nano zinc oxide in the porous filler, and increases the mechanical properties of the PVC sports flooring by the high dispersibility of the porous filler.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] The utility model relates to a PVC sports flooring, which consists of a base fabric, a foaming layer, a surface layer and a PVC layer from bottom to top.
[0009] The foaming layer comprises the following components by weight: 80-120 parts of polyvinyl chloride paste resin, 54-68 parts of porous filler, 60-70 parts of plasticizer, 1-2 parts of potassium zinc stabilizer, and 6-10 parts of foaming agent.
[0010] The porous filler is prepared by the following steps:
[0011] Dissolve Zn(NO3)2·4H2O and terephthalic acid in N,N-dimethylformamide at 70-75°C, stir for 70-72 hours, then heat to 105-110°C to produce precipitation, then cool to 30-35°C to crystallize for 18-24 hours, filter after crystallization, wash with N,N-dimethylformamide, toluene, and ethanol in turn, and vacuum dry at 45-55°C to obtain a porous carrier, disperse the porous carrier in methanol, add nano zinc oxide, and then stir at 55-65°C until the methanol is completely volatilized to obtain a porous filler.
[0012] Furthermore, the surface layer comprises the following components by weight: 80-120 parts of polyvinyl chloride paste resin, 60-70 parts of plasticizer, 1-2 parts of potassium zinc stabilizer, and 30-35 parts of nano calcium carbonate.
[0013] Furthermore, the PVC layer comprises the following components by weight: 80-100 parts of polyvinyl chloride resin, 55-65 parts of plasticizer and 1-2 parts of potassium zinc stabilizer.
[0014] Furthermore, the plasticizer is dioctyl phthalate, and the foaming agent is azodicarbonamide.
[0015] Furthermore, the mass ratio of the porous carrier to the nano zinc oxide is 25-30:2-4.
[0016] Furthermore, the usage ratio of Zn(NO3)2·4H2O, terephthalic acid and N,N-dimethylformamide is 3-3.5g:0.7-0.8g:100-110mL.
[0017] A method for preparing PVC sports flooring comprises the following steps:
[0018] Step 1: Apply the foaming layer slurry on the base fabric with a coating amount of 800-1200g / m 2 , cure at 140-150℃ for 55-75s, cool, then cure at 80-120g / m 2 The surface slurry is applied on the surface of the solidified foaming layer with a sizing amount, and cured at 140-150°C for 25-35s to obtain the pre-foamed floor glue.
[0019] Step 2: Send the pre-foamed floor glue into a foaming furnace for foaming, so that the foaming layer is foamed to 4-8mm to obtain the foamed floor glue.
[0020] Step 3: Mix the polyvinyl chloride resin, plasticizer and potassium zinc stabilizer, melt them at 180-185℃ and apply them on the surface of the foam flooring with a coating machine. The coating amount is 40-60g / m 2 After cooling and shaping, it is cut and embossed to obtain PVC sports flooring.
[0021] Further, the foaming layer slurry is prepared by the following steps:
[0022] The polyvinyl chloride paste resin and the foaming agent are stirred evenly to obtain the foaming resin, and the porous filler is dispersed in the slurry barrel with ethanol. After dispersion, the plasticizer and the potassium zinc stabilizer are added. The mixture is heated in a water bath to 50-60°C and stirred until the ethanol is completely volatilized. Then, the foaming resin is added to the slurry barrel and dispersed at a speed of 1200-1600rpm for 1-2h to obtain the foaming layer slurry.
[0023] Further, the surface slurry is prepared by the following steps:
[0024] The polyvinyl chloride paste resin, plasticizer, potassium zinc stabilizer and nano calcium carbonate are mixed, and dispersed at a speed of 1600-1800 rpm for 20-40 minutes to obtain a surface layer slurry.
[0025] Furthermore, in step 2, the foaming furnace includes four zones, the temperature of the first zone is 190-200°C, the temperature of the second zone is 190-210°C, the temperature of the third zone is 200-220°C, and the temperature of the fourth zone is 160-200°C.
[0026] Beneficial effects of the present invention:
[0027] (1) The porous filler added to the foaming layer of the present invention causes the bubbles generated by the foaming agent in the foaming layer to generate uniform and fine bubbles through the high specific surface area of the porous filler, so that the foaming structure is more uniform and the bubble structure is denser. The bubbles in the foaming layer formed are uniform and dense, and have excellent shock-absorbing performance. At the same time, the porous filler has a high dispersibility in the PVC paste resin because it contains carboxyl groups. The porous filler improves the wear resistance and mechanical properties of the PVC paste resin, thereby improving the mechanical properties of the PVC sports flooring.
[0028] (2) The present invention dissolves nano zinc oxide in methanol and mixes the nano zinc oxide in the porous structure of the porous carrier. The nano zinc oxide can provide more active sites for the foaming agent, which can significantly affect the decomposition rate of the foaming agent, reduce the reaction activation energy, reduce the foaming temperature, and increase the foaming rate, so that the bubbles have enough time to be evenly dispersed in the foaming layer, thereby improving the toughness of the foaming layer and the shock absorption performance of the sports flooring.
[0029] (2) In the preparation method of the present invention, by mixing the porous filler loaded with nano zinc oxide with the plasticizer, part of the plasticizer is filled in the porous filler, which reduces the migration of the plasticizer to the surface of the foaming layer, and the obtained foaming layer has good flexibility. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1: A PVC sports flooring comprises, from bottom to top, a base fabric, a foaming layer, a surface layer and a PVC layer.
[0032] A method for preparing PVC sports flooring comprises the following steps:
[0033] Step 1: Apply the foaming layer slurry on the base fabric with a coating amount of 800g / m 2 , cured at 140°C for 55 seconds, cooled, and then cured at 80 g / m 2 The surface slurry is applied on the surface of the solidified foaming layer with a sizing amount, and cured at 140°C for 25s to obtain the pre-foamed floor glue.
[0034] Step 2: Send the pre-foamed floor glue into a foaming furnace for foaming, so that the foaming layer is foamed to 4mm to obtain the foamed floor glue.
[0035] Step 3: Mix 80g polyvinyl chloride resin, 55g dioctyl phthalate and 1g potassium zinc stabilizer, melt at 180℃ and apply it on the surface of the foam flooring with a coating machine. The coating amount is 40g / m 2 After cooling and shaping, it is cut and embossed to obtain PVC sports flooring.
[0036] The foaming furnace includes four zones, the temperature of the first zone is 190°C, the temperature of the second zone is 190°C, the temperature of the third zone is 200°C, and the temperature of the fourth zone is 160°C.
[0037] The foaming layer slurry is prepared by the following steps:
[0038] 800g of polyvinyl chloride paste resin and 60g of azodicarbonamide were stirred to obtain foaming resin, 540g of porous filler was dispersed in a slurry barrel with 1L of ethanol, 600g of dioctyl phthalate and 10g of potassium zinc stabilizer were added after dispersion, and a water bath was heated to 50°C and stirred until the ethanol was completely volatilized, and then the foaming resin was added to the slurry barrel and dispersed at a speed of 1200rpm for 1h to obtain a foaming layer slurry.
[0039] The surface slurry is prepared by the following steps:
[0040] 80 g of polyvinyl chloride paste resin, 60 g of dioctyl phthalate, 1 g of potassium zinc stabilizer and 30 g of nano calcium carbonate were mixed and dispersed at a speed of 1600 rpm for 20 minutes to obtain a surface layer slurry.
[0041] The degree of polymerization of the polyvinyl chloride paste resin is 1000.
[0042] The porous filler is prepared by the following steps:
[0043] 900g Zn(NO3)2·4H2O and 210g terephthalic acid were dissolved in 30L N,N-dimethylformamide at 70°C, stirred for 70 hours, then heated to 105°C to produce precipitation, then cooled to 35°C for crystallization for 18h, filtered after crystallization, washed with N,N-dimethylformamide, toluene, and ethanol in turn, and vacuum dried at 45°C to obtain a porous carrier. 500g of the porous carrier was dispersed in 1L methanol, 40g of nano zinc oxide was added, and then stirred at 55°C until the methanol was completely volatilized to obtain a porous filler.
[0044] Example 2
[0045] The utility model relates to a PVC sports flooring, which comprises a base fabric, a foaming layer, a surface layer and a PVC layer from bottom to top.
[0046] A method for preparing PVC sports flooring comprises the following steps:
[0047] Step 1: Apply the foaming layer slurry on the base fabric with a coating amount of 1000g / m 2 , cured at 145°C for 65s, cooled, and then 2 The surface slurry is applied on the surface of the solidified foaming layer with a sizing amount, and cured at 145°C for 30s to obtain the pre-foamed floor glue.
[0048] Step 2: Send the pre-foamed floor glue into a foaming furnace for foaming, so that the foaming layer is foamed to 6mm to obtain the foamed floor glue.
[0049] Step 3: Mix 90g of polyvinyl chloride resin, 60g of dioctyl phthalate and 1.5g of potassium zinc stabilizer, melt at 183°C and apply it on the surface of the foam flooring with a coating machine. The coating amount is 50g / m 2 After cooling and shaping, it is cut and embossed to obtain PVC sports flooring.
[0050] The foaming furnace includes four zones, the temperature of the first zone is 195°C, the temperature of the second zone is 200°C, the temperature of the third zone is 210°C, and the temperature of the fourth zone is 180°C.
[0051] The foaming layer slurry is prepared by the following steps:
[0052] 1000g of polyvinyl chloride paste resin and 80g of azodicarbonamide were stirred to obtain foaming resin. 600g of porous filler was dispersed in a slurry barrel with 1L of ethanol. After dispersion, 650g of dioctyl phthalate and 15g of potassium zinc stabilizer were added. The mixture was heated to 55°C in a water bath and stirred until the ethanol was completely evaporated. Then, the foaming resin was added to the slurry barrel and dispersed at a speed of 1400rpm for 1.5h to obtain a foaming layer slurry.
[0053] The surface slurry is prepared by the following steps:
[0054] 100 g of polyvinyl chloride paste resin, 65 g of dioctyl phthalate, 1.5 g of potassium zinc stabilizer and 33 g of nano calcium carbonate were mixed and dispersed at a speed of 1700 rpm for 30 minutes to obtain a surface layer slurry.
[0055] The degree of polymerization of polyvinyl chloride paste resin is 1300.
[0056] The porous filler is prepared by the following steps:
[0057] 1000g Zn(NO3)2·4H2O and 225g terephthalic acid were dissolved in 31L N,N-dimethylformamide at 73°C, stirred for 71 hours, then heated to 108°C to produce precipitation, then cooled to 33°C for crystallization for 21 hours, filtered after crystallization, washed with N,N-dimethylformamide, toluene, and ethanol in turn, and vacuum dried at 50°C to obtain a porous carrier. 550g of the porous carrier was dispersed in 1L methanol, 60g of nano zinc oxide was added, and then stirred at 60°C until the methanol was completely volatilized to obtain a porous filler.
[0058] Embodiment 3: A PVC sports flooring comprises, from bottom to top, a base fabric, a foaming layer, a surface layer and a PVC layer.
[0059] A method for preparing PVC sports flooring comprises the following steps:
[0060] Step 1: Apply the foaming layer slurry on the base fabric with a coating amount of 1200g / m 2 , cured at 150°C for 75 seconds, cooled, and then cured at 120 g / m 2 The surface slurry is applied on the surface of the cured foaming layer with a sizing amount, and cured at 150°C for 35s to obtain the pre-foamed floor glue.
[0061] Step 2: Send the pre-foamed floor glue into a foaming furnace for foaming, so that the foaming layer is foamed to 8mm to obtain the foamed floor glue.
[0062] Step 3: Mix 100g polyvinyl chloride resin, 65g dioctyl phthalate and 2g potassium zinc stabilizer, melt at 185℃ and apply it on the surface of the foam floor with a coating machine. The coating amount is 60g / m 2 After cooling and shaping, it is cut and embossed to obtain PVC sports flooring.
[0063] The foaming furnace includes four zones, the temperature of the first zone is 200°C, the temperature of the second zone is 210°C, the temperature of the third zone is 220°C, and the temperature of the fourth zone is 200°C.
[0064] The foaming layer slurry is prepared by the following steps:
[0065] 1200g of polyvinyl chloride paste resin and 100g of azodicarbonamide were stirred to obtain foaming resin, 680g of porous filler was dispersed in a slurry barrel with 1L of ethanol, 700g of dioctyl phthalate and 20g of potassium zinc stabilizer were added after dispersion, and a water bath was heated to 60°C and stirred until the ethanol was completely volatilized. Then, the foaming resin was added to the slurry barrel and dispersed at a speed of 1600rpm for 2h to obtain a foaming layer slurry.
[0066] The surface slurry is prepared by the following steps:
[0067] 120 g of polyvinyl chloride paste resin, 70 g of dioctyl phthalate, 2 g of potassium zinc stabilizer and 35 g of nano calcium carbonate were mixed and dispersed at a speed of 1800 rpm for 40 minutes to obtain a surface layer slurry.
[0068] The degree of polymerization of the polyvinyl chloride paste resin is 1500.
[0069] The porous filler is prepared by the following steps:
[0070] 1050g Zn(NO3)2·4H2O and 240g terephthalic acid were dissolved in 33L N,N-dimethylformamide at 75°C, stirred for 72 hours, then heated to 110°C to produce precipitation, then cooled to 35°C for crystallization for 24 hours, filtered after crystallization, washed with N,N-dimethylformamide, toluene, and ethanol in turn, and vacuum dried at 55°C to obtain a porous carrier. 600g of the porous carrier was dispersed in 1L methanol, 80g of nano zinc oxide was added, and then stirred at 65°C until the methanol was completely volatilized to obtain a porous filler.
[0071] Principle of the invention:
[0072] By adding porous fillers in the foaming layer, the specific surface area of the fillers in the foaming layer is increased, so that the bubbles generated when the foaming agent foams are distributed more evenly through the porous structure, forming a denser bubble structure.
[0073] The present invention dissolves nano zinc oxide by methanol, so that the nano zinc oxide is mixed in the porous structure of a porous carrier. The nano zinc oxide can provide more active sites for a foaming agent, can significantly affect the decomposition rate of the foaming agent, reduce the reaction activation energy, reduce the foaming temperature, and increase the foaming rate, so that the bubbles have enough time to be evenly dispersed in the foaming layer. Under the action of the porous filler loaded with nano zinc oxide, the foaming layer of the sports flooring can have dense pores and uniform foaming, thereby improving the toughness of the foaming layer and the shock absorbing performance of the sports flooring.
[0074] In the porous carrier structure synthesized by terephthalic acid of the present invention, the carboxyl group in the terephthalic acid makes the porous carrier have good dispersibility in the PVC paste resin, so that the porous carrier is dispersed in the PVC paste resin, which can make the foaming agent contact with the porous carrier evenly in the foaming layer and improve the uniformity of bubble dispersion, and can also be used as a filler to improve the wear resistance and mechanical properties of the foaming layer.
[0075] Phthalate plasticizers can easily migrate from PVC products to the surface of PVC. In the present invention, the porous filler loaded with nano zinc oxide is dispersed with ethanol and then mixed with the plasticizer to fill part of the porous filler with the plasticizer, thereby reducing the migration of the plasticizer to the surface of the foaming layer.
[0076] Comparative Example 1: The difference from Example 1 is that in the foaming layer slurry, a porous filler is used instead of the porous filler loaded with nano zinc oxide.
[0077] Comparative Example 2: The difference from Example 1 is that in the foaming layer slurry, an equal mass of nano calcium carbonate is used to replace the porous filler loaded with nano zinc oxide.
[0078] Comparative Example 3: The difference from Example 1 is that the porous filler is prepared using the following steps:
[0079] In a reactor, 900g of AI(NO3)3·9H20 was dispersed in 7L of distilled water, 170g of terephthalic acid was dissolved in 5L of N,N-dimethylformamide, then added to the reactor and stirred for 30min, poured into a high-pressure reactor and hydrothermal at 180°C for 8h, then taken out, the surface of the substrate was rinsed with distilled water and N,N-dimethylformamide in turn, and then dried at 60°C for 12h to obtain a porous carrier, 500g of the porous carrier was dispersed in 1L of methanol, 40g of nano zinc oxide was added, and then stirred at 55°C until the methanol was completely volatilized to obtain a porous filler.
[0080] Sources of reagents in Examples and Comparative Examples:
[0081] Polyvinyl chloride paste resin was purchased from Jiangsu Bosite Chemical Technology Co., Ltd.;
[0082] Nano zinc oxide was purchased from Shanghai Hanlang New Material Technology Co., Ltd.;
[0083] Nano Calcium Carbonate Shanghai Hanlang New Material Technology Co., Ltd.;
[0084] Potassium zinc stabilizer was purchased from Shenzhen Jielitai Plastic Products Co., Ltd.;
[0085] Dioctyl phthalate, azodicarbonamide, Zn(NO3)2·4H2O, AI(NO3)3·9H20, terephthalic acid, and N,N-dimethylformamide were purchased from Sigma Aldrich.
[0086] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. The shock energy absorption rate was tested according to EN 14808-2005, and the tensile strength and elongation at break were tested according to GB / T14833-20206.6. The results are shown in Table 1:
[0087] Table 1
[0088] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Shock energy absorption rate% 19.7 21.2 24.6 15.7 14.4 17.5 Tensile strengthMpa 4.32 4.67 4.81 3.18 3.05 3.94 Elongation at break % 154 162 167 141 134 146
[0089] As can be seen from Table 1, the shock energy absorption rate of the PVC sports flooring obtained in Examples 1 to 3 is high compared with that in Comparative Examples 1 to 3, indicating that the foaming layer prepared in the present invention has a good bubble structure and a high shock energy absorption rate. Since the foaming thickness of the foaming layer is different in Examples 1 to 3, the shock energy absorption rate will also increase with the increase of the foaming thickness. In Comparative Example 1, due to the addition of porous fillers, the specific surface area of the porous filler is greater than that of the nano-calcium carbonate in Comparative Example 2, and the shock energy absorption rate of Comparative Example 1 is slightly greater than that of Comparative Example 2; the test performance of Comparative Example 3 is slightly worse than that of Example 1, indicating that the addition of fillers with porous structures is conducive to the formation of PVC sports flooring with excellent performance. The reason why the test performance of the PVC sports flooring obtained in Comparative Example 3 is poor is that the pore structure of the porous filler is different and the raw materials of the porous filler are different. The porous filler in the embodiment is Zn element, and the porous filler formed by the Zn element may have a better activation effect on the foaming agent, so that the performance of the PVC sports flooring in Example 1 is better than that of Comparative Example 3.
[0090] The tensile strength and elongation at break obtained in Examples 1 to 3 are greater than those in Comparative Examples 1 and 3, indicating that the PVC sports flooring obtained in the present invention has good toughness and the honeycomb structure formed by foaming is evenly distributed.
[0091] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A PVC sports flooring, characterized in that: The PVC sports flooring is composed of a base fabric, a foaming layer, a surface layer and a PVC layer from bottom to top; The foaming layer comprises the following components by weight: 80-120 parts of polyvinyl chloride paste resin, 54-68 parts of porous filler, 60-70 parts of plasticizer, 1-2 parts of potassium zinc stabilizer, and 6-10 parts of foaming agent; The porous filler is prepared by the following steps: Dissolve Zn(NO3)2·4H2O and terephthalic acid in N,N-dimethylformamide at 70-75°C, stir for 70-72 hours, then heat to 105-110°C to produce precipitation, then cool to 30-35°C to crystallize for 18-24 hours, filter after crystallization, wash with N,N-dimethylformamide, toluene, and ethanol, and dry in vacuum at 45-55°C to obtain a porous carrier; The porous carrier is dispersed in methanol, nano zinc oxide is added, and then stirred at 55-65° C. until the methanol is completely volatilized to obtain a porous filler.
2. A PVC sports flooring according to claim 1, characterized in that: The surface layer comprises the following components by weight: 80-120 parts of polyvinyl chloride paste resin, 60-70 parts of plasticizer, 1-2 parts of potassium zinc stabilizer, and 30-35 parts of nano calcium carbonate; The PVC layer comprises the following components by weight: 80-100 parts of polyvinyl chloride resin, 55-65 parts of plasticizer and 1-2 parts of potassium zinc stabilizer; The plasticizer is dioctyl phthalate.
3. The PVC sports flooring according to claim 1, characterized in that: The foaming agent is azodicarbonamide.
4. The PVC sports flooring according to claim 1, characterized in that: The mass ratio of the porous carrier to the nano zinc oxide is 25-30:2-4.
5. The PVC sports flooring according to claim 1, characterized in that: The usage ratio of Zn(NO3)2·4H2O, terephthalic acid and N,N-dimethylformamide is 3-3.5g:0.7-0.8g:100-110mL.
6. The method for preparing a PVC sports flooring according to claim 1, characterized in that: The steps include: Step 1: Apply the foaming layer slurry on the base fabric with a coating amount of 800-1200g / m 2 , cure at 140-150℃ for 55-75s, cool, then cure at 80-120g / m 2 Apply the surface slurry on the surface of the solidified foaming layer with a sizing amount of sizing, and solidify it at 140-150°C for 25-35s to obtain the pre-foamed floor glue; Step 2: Send the pre-foamed floor glue into a foaming furnace for foaming, so that the foaming layer is foamed to 4-8mm to obtain a foamed floor glue; Step 3: Mix the polyvinyl chloride resin, plasticizer and potassium zinc stabilizer, melt them at 180-185℃ and apply them on the surface of the foam flooring with a coating machine. The coating amount is 40-60g / m 2 After cooling and shaping, it is cut and embossed to obtain PVC sports flooring.
7. The method for preparing a PVC sports flooring according to claim 6, characterized in that: The foaming layer slurry is prepared by the following steps: The polyvinyl chloride paste resin and the foaming agent are stirred evenly to obtain the foaming resin, and the porous filler is dispersed in the slurry barrel with ethanol. After dispersion, the plasticizer and the potassium zinc stabilizer are added. The mixture is heated in a water bath to 50-60°C and stirred until the ethanol is completely volatilized. Then, the foaming resin is added to the slurry barrel and dispersed at a speed of 1200-1600rpm for 1-2h to obtain the foaming layer slurry.
8. The method for preparing a PVC sports flooring according to claim 6, characterized in that: The surface layer slurry is prepared by the following steps: The polyvinyl chloride paste resin, plasticizer, potassium zinc stabilizer and nano calcium carbonate are mixed, and dispersed at a speed of 1600-1800 rpm for 20-40 minutes to obtain a surface layer slurry.
9. The method for preparing a PVC sports flooring according to claim 6, characterized in that: The foaming furnace in step 2 includes four zones, the temperature of the first zone is 190-200°C, the temperature of the second zone is 190-210°C, the temperature of the third zone is 200-220°C, and the temperature of the fourth zone is 160-200°C.
Citation Information
Patent Citations
Metal-organic framework nanocrystal loaded polyurethane foam as well as preparation and application thereof
CN106366636A
Microcellular foamed PVC wallpaper
CN108948598A
Environment-friendly flame-retardant floor leather
CN109868658A
Sound insulation board for road and preparation method of sound insulation board
CN118185288A
Metal MOF functional complex modified polylactic acid as well as preparation method and application thereof
CN118290916A