Method for simultaneously self-assembling and growing multifunctional micro-nano array
By combining a bottom-up self-assembly growth method with phase change materials, the problem of repetitive patterning steps in the fabrication of multifunctional micro- and nano-arrays has been solved, enabling low-cost and high-efficiency fabrication of multifunctional micro- and nano-arrays suitable for applications such as high-resolution full-color imaging and information storage.
Patent Information
- Application Number
- CN202410897105.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies require repeated patterning steps when fabricating multifunctional micro/nano arrays, resulting in high production costs, low yields, and difficulty in scaling up, especially for organic materials that are susceptible to environmental influences.
A bottom-up self-assembly growth method combined with phase change materials is adopted to complete the fabrication of multifunctional micro-nano arrays in one step through surface modification, photolithography, etching, self-assembly and annealing. Multifunctional micro-nano arrays are formed by using phase change materials in different crystal states.
It simplifies the fabrication process, reduces costs, improves production efficiency, and enables the scalability of high-quality, multifunctional micro-nano arrays, suitable for applications such as high-resolution full-color imaging, photonic crystals, and information storage.
Smart Images

Figure CN118929564A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micro-nano processing, and in particular relates to a method for growing a multifunctional micro-nano array. Background Art
[0002] Multifunctional micro-nano arrays with different pixel types hold great promise in various applications, such as high-resolution full-color imaging / display, photonic crystals, information storage, encryption, etc. Currently, the development of multifunctional micro-nano arrays with different pixel types requires continuous and repeated patterning steps of different materials. For example, techniques such as inkjet printing, transfer printing, and selective electrophoretic deposition are used to sequentially pattern different materials on the same substrate. However, these cyclically repeated patterning techniques increase production costs and reduce yields, especially for organic materials that are susceptible to environmental influences. Limited scalability and difficulty in integration are also major issues for various technologies. Therefore, there is an urgent need to develop a simple method for preparing multifunctional micro-nano arrays in one step or fewer steps. Summary of the invention
[0003] The purpose of the present invention is to provide a method for simultaneously self-assembling and growing a multifunctional micro-nano array, so as to improve the growth quality and simplify the growth process.
[0004] The method for simultaneous self-assembly growth of multifunctional micro-nano arrays provided by the present invention comprises the following specific steps:
[0005] (1) performing surface modification on the substrate to form a modified layer;
[0006] (2) performing photolithography on the modified layer to form a photoresist pattern;
[0007] (3) transferring the photoresist pattern to the modification layer by etching, stripping and other steps to form modification layer patterns of different sizes or the same size but different surface energies;
[0008] (4) performing self-assembly growth of phase change material on the modification layer pattern to form amorphous patterns (nucleation sites) of phase change material of different sizes or containing different amounts of substances;
[0009] (5) Annealing treatment is performed to transform the amorphous pattern with a larger mass into a crystalline state, while the amorphous pattern with a smaller mass remains in an amorphous state, thereby realizing a multifunctional micro-nano array.
[0010] Optionally, the substrate is one of a rigid substrate and a flexible substrate, specifically selected from silicon oxide, silicon, glass, PET, and PI.
[0011] Optionally, the method for modifying the surface of the substrate is selected from one of gas phase evaporation and solution immersion. The material of the modification layer is selected from one of OTS, FTS, FAS, HMDS and PDMS.
[0012] Optionally, the photolithography is selected from one of ultraviolet photolithography, laser direct writing and electron beam lithography.
[0013] Optionally, the self-assembly growth is selected from one of vapor phase self-assembly growth and wet self-assembly growth. The vapor phase self-assembly growth is carried out under ultra-high vacuum conditions, and the phase change material is deposited on the surface of the substrate after heating and sublimation, and a pattern is formed based on the difference in binding energy between the phase change material, the substrate and the modified layer. The wet self-assembly growth is selected from one of drip coating, scraping, dip-pull and printing. The drip coating is to drop the phase change material solution on the substrate in the form of droplets, and form a pattern by using the difference in contact angles between the solvent, the substrate and the modified layer. The scraping is to move the scraper on the surface at a certain inclination angle, and use shear force to induce the phase change material solution to form a film on the substrate with the modified layer pattern. The dip-pull is to immerse the substrate with the modified layer pattern in the phase change material solution and then pull it out at a certain speed, and the solution diffuses and evaporates to form a film. The printing is to directly print the phase change material solution on the substrate, and the pattern is formed after the solvent evaporates.
[0014] The phase change material can be selected from aggregation-induced emission (AIE) materials such as 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenyl acetate (NITPAC1), 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenyl octanoate (NITPAC4), 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)anisole (NITPA1), and 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenylethyl ether (NITPA2).
[0015] The present invention also provides a multifunctional micro-nano array, comprising: a substrate; a modification layer pattern of different sizes or the same size but different surface energies obtained by programmatic control on the same substrate surface through photolithography technology (a phase change material that can adsorb different amounts of matter); a multifunctional micro-nano array composed of a crystalline state with a larger amount of matter and an amorphous state pattern with a smaller amount of matter on the modification layer pattern.
[0016] The present invention combines the bottom-up self-assembly growth patterning strategy with phase change materials to realize a multifunctional micro-nano array composed of phase change materials in different crystal states. Compared with the traditional cyclic repetitive patterning technology, it has the advantages of simple process, low cost, strong scalability, etc., and can obtain high-quality micro-nano arrays, which can be applied to high-resolution full-color imaging / display, photonic crystals, information storage, encryption and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a flow chart of the method for simultaneously self-assembling and growing multifunctional micro-nano arrays.
[0018] Figure 2A-2F The process flow chart of the method of the present invention is shown in FIG.
[0019] Figure 3 Optical microscopic characterization photographs of amorphous dot arrays with diameters of 8 μm and 25 μm produced in the examples.
[0020] Figure 4 Yes Figure 3 Optical microscopic characterization photographs of the NITPAC1 multifunctional array obtained after annealing, with the 25μm diameter dots being crystalline and the 8μm diameter dots being amorphous.
[0021] Figure 5 Yes Figure 4 Photoluminescence spectra of dots with different diameters. DETAILED DESCRIPTION
[0022] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings.
[0023] Figure 1 The figure is a schematic diagram of the implementation steps of the method described in this specific embodiment, including:
[0024] Step S10, providing a substrate;
[0025] Step S11, performing surface modification on the substrate to form a modified layer;
[0026] Step S12, performing photolithography on the modified layer to form a photoresist pattern;
[0027] Step S13, transferring the photoresist pattern to the modification layer by etching, stripping and other steps to form modification layer patterns of different sizes or the same size but different surface energies;
[0028] Step S14, performing self-assembly growth of phase change material on the modification layer pattern to form amorphous patterns (nucleation sites) of phase change material of different sizes or containing different amounts of substances;
[0029] Step S15, performing annealing treatment to transform the amorphous pattern with a larger mass into a crystalline state, while the amorphous pattern with a smaller mass remains in an amorphous state, thereby realizing a multifunctional micro-nano array.
[0030] Figure 2A As shown, referring to step S10, a substrate 20 is provided. The substrate 20 is selected from a rigid substrate and a flexible substrate. In this specific embodiment, it is a silicon oxide substrate.
[0031] Figure 2B As shown, referring to step S11, the substrate 20 is surface modified to form a modified layer 21. The method for surface modification of the substrate 20 is selected from one of gas phase evaporation and solution immersion. In this specific embodiment, the solution immersion method is adopted, and the modified layer 21 is OTS.
[0032] Figure 2C As shown, referring to step S12, photolithography is performed on the modified layer 21 to form a photoresist 22 pattern. The photolithography is selected from one of ultraviolet lithography, laser direct writing and electron beam lithography. In this specific embodiment, ultraviolet lithography is adopted, and the specific steps include spin coating photoresist, pre-baking, exposure, development and post-baking, etc.
[0033] Figure 2D As shown, referring to step S13, the photoresist 22 pattern is transferred to the modification layer 21 by etching, stripping and other steps to form the modification layer 21 patterns of different sizes or the same size with different surface energies. In this specific embodiment, etching is performed by oxygen plasma etching, and stripping is performed by immersing the sample in acetone.
[0034] Figure 2E As shown, referring to step S14, self-assembly growth of phase change material is carried out on the pattern of the modification layer 21 to form amorphous phase change material patterns 23 of different sizes or containing different amounts of substances (nucleation sites). The self-assembly growth is selected from one of vapor phase self-assembly growth and wet self-assembly growth. The wet self-assembly growth is selected from one of drip coating, scraping, dip-pull and printing. In this specific embodiment, dip-pull in wet self-assembly growth is adopted. In the dip-pull process, the substrate with the modification layer pattern is immersed in the phase change material solution and then pulled out at a certain speed, and the solution diffuses and evaporates to form a film.
[0035] Figure 2F As shown, referring to step S15, annealing treatment is performed to transform the amorphous state 23 pattern with a larger amount of substance into a crystalline state 24, while the amorphous state 23 pattern with a smaller amount of substance remains in an amorphous state, thereby realizing a multifunctional micro-nano array. The annealing treatment step is to place the sample in an inert gas or vacuum atmosphere for heating.
[0036] After the above steps are completed, a multifunctional micro-nano array is obtained, including: a substrate 20; a modification layer 21 pattern of different sizes or the same size but different surface energies obtained by programmatic control on the surface of the same substrate 20 by means of photolithography technology (phase change materials that can adsorb different amounts of substances); a multifunctional micro-nano array composed of a crystalline state 24 with a larger amount of substance and an amorphous state 23 pattern with a smaller amount of substance on the modification layer 21 pattern.
[0037] An embodiment of the present invention is given below.
[0038] The phase change material of this embodiment adopts the aggregation-induced emission (AIE) material 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinolin-2(3H)-yl)phenyl acetate (NITPAC1), and its structural formula is:
[0039]
[0040] The specific steps for preparing the multifunctional micro-nano array are as follows:
[0041] (1) The silicon oxide substrate was immersed in acetone, isopropanol and deionized water for 30 minutes each, and then dried with a nitrogen gun.
[0042] (2) The silicon oxide substrate was immersed in a mixed solution of OTS, dichloromethane and n-hexane (volume ratio 1:375:500) for 10 minutes to complete the OTS surface modification.
[0043] (3) Spin-coating photoresist on the modification layer OTS (S1805), and obtaining a photoresist pattern through the steps of pre-baking, exposure, development and post-baking. The photoresist pattern is a dot array with two sizes, large and small, where the diameter of the large-sized dot is 25 μm and the diameter of the small-sized dot is 8 μm.
[0044] (4) The OTS in the dot array is etched away using oxygen plasma etching, and then the sample is immersed in acetone to remove the adhesive to obtain the OTS pattern.
[0045] (5) NITPAC1 powder was dissolved in dichloromethane to prepare a solution with a concentration of 15 mg / mL. The OTS-patterned silicon oxide substrate was immersed in the solution and heated at 100 μm s -1 During the pulling process, microdroplets were formed in the OTS-free area, and after the dichloromethane evaporated, two sizes of NITPAC1 amorphous dot arrays were obtained.
[0046] (6) Annealing treatment was performed to transform the 25 μm diameter NITPAC1 amorphous dots into a crystalline state by controlling the annealing temperature and time, while the 8 μm diameter amorphous dots remained amorphous, thereby realizing a multifunctional micro-nano array. The annealing environment was a nitrogen atmosphere, the temperature was 100°C, and the time was 1 hour.
[0047] The NITPAC1 dot arrays with diameters of 8 μm and 25 μm prepared in this example were characterized by optical microscopy. Figure 3 , 4 shown. Figure 3 The NITPAC1 dot arrays of two sizes were amorphous before annealing. Figure 4 The NITPAC1 multifunctional array is obtained after annealing, with the 25 μm diameter dots being crystalline and the 8 μm diameter dots being amorphous. Figure 4 The NITPAC1 multifunctional array was characterized by spectroscopy, and the photoluminescence spectra of dots with different diameters were obtained, such as Figure 5 shown.
[0048] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for simultaneously self-assembling and growing a multifunctional micro-nano array, characterized in that: The specific steps are: (1) performing surface modification on the substrate to form a modified layer; (2) performing photolithography on the modified layer to form a photoresist pattern; (3) transferring the photoresist pattern to the modification layer by etching, stripping and other steps to form modification layer patterns of different sizes or the same size but different surface energies; (4) performing self-assembly growth of phase change material on the modification layer pattern to form amorphous patterns (nucleation sites) of phase change material of different sizes or containing different amounts of substances; (5) Annealing treatment is performed to transform the amorphous pattern with a larger mass into a crystalline state, while the amorphous pattern with a smaller mass remains in an amorphous state, thereby realizing a multifunctional micro-nano array.
2. The method according to claim 1, characterized in that In step (1): The substrate is one of a rigid substrate and a flexible substrate; The method for surface modification of the substrate is selected from one of gas phase evaporation and solution immersion; The material of the modification layer is selected from one of OTS, FTS, FAS, HMDS and PDMS.
3. The method according to claim 1, characterized in that The photolithography in step (2) is selected from one of ultraviolet photolithography, laser direct writing and electron beam lithography.
4. The method according to claim 1, characterized in that: The self-assembly growth in step (4) is selected from one of vapor phase self-assembly growth and wet self-assembly growth; The gas phase self-assembly growth is carried out under ultra-high vacuum conditions, the phase change material is heated and sublimated and then deposited on the substrate surface, and a pattern is formed based on the difference in binding energy between the phase change material, the substrate and the modified layer; The wet self-assembly growth is selected from one of drop coating, scraping, immersion pulling and printing; the drop coating is to drop the phase change material solution on the substrate in the form of droplets, and form a pattern by utilizing the difference in contact angles between the solvent and the substrate and the modified layer; The scraping method is to move the scraper on the surface at a certain inclination angle, and use shear force to induce the phase change material solution to form a film on the substrate with the modification layer pattern; the immersion pulling method is to immerse the substrate with the modification layer pattern into the phase change material solution and then pull it out at a certain speed, and the solution diffuses and evaporates to form a film; the printing method is to directly print the phase change material solution on the substrate, and a pattern is formed after the solvent evaporates.
5. The method according to claim 4, characterized in that The phase change material in step (4) is selected from the aggregation-induced emission (AIE) material 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenyl acetate (NITPAC1), 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenyl octanoate (NITPAC4), 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)anisole (NITPA1) or 3-(6-(4-(diphenylamino)phenyl)-1,3-dioxa-1H-benzo[iso]quinoline-2(3H)-yl)phenylethyl ether (NITPA2).
6. A multifunctional micro-nano array obtained by the method according to any one of claims 1 to 5, comprising: substrate; The substrate surface is programmed to obtain modified layer patterns of different sizes or the same size but different surface energies by photolithography, and the modified layer patterns adsorb phase change materials of different material quantities; A multifunctional micro-nano array is formed by a crystalline state with a larger amount of substance and an amorphous state pattern with a smaller amount of substance on the modification layer pattern.