Protruding micro-nano feature machining process based on amorphous alloy
Through a processing technology based on amorphous alloys, nano-scale polishing and lithography technology are used to form pattern templates, combined with magnetron sputtering and heating treatment, the accuracy and cost problems in traditional micro-nano feature processing are solved, and high efficiency and low cost are achieved. The raised micro-nano feature processing significantly improves the stability and wear resistance of micro-nano devices.
Patent Information
- Application Number
- CN202411002031.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional micro-nano feature processing technology is difficult to ensure high accuracy and low cost when processing raised micro-nano features, and is susceptible to the impact of cutting forces and thermal stresses to cause structure collapse and deformation, making it difficult to meet the needs of large-scale production.
Using a processing technology based on amorphous alloy, pattern templates are formed through nano-scale polishing and photolithography technology, magnetron sputtering is used to activate the amorphous alloy and spray it, forming uniformly raised micro-nano features only in the exposed area, and heating is used to make The amorphous alloy crystallization enhances the bonding force between the coating and the substrate.
It improves processing accuracy and efficiency, reduces production costs, significantly enhances the stability and wear resistance of the raised micro-nano features, and extends the service life of micro-nano devices.
Smart Images

Figure CN118929567A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precision machining, and in particular to a protruding micro-nano feature machining process based on amorphous alloys. Background Art
[0002] With the rapid development of science and technology, micro-nano technology has become an important force in promoting the progress of modern industry. As the core component of micro-nano technology, metal micro-nano devices have shown broad application prospects in micro-nano electronics, optoelectronics, biomedicine and precision machinery due to their unique physical and chemical properties and high-precision three-dimensional structure. The performance of these devices often directly depends on the accuracy and stability of their micro-nano structures, especially the raised micro-nano features, which play a vital role in realizing the specific functions of the devices.
[0003] Traditional micro-nano feature processing technologies mainly rely on precision machine tool processing technologies for the processing of raised micro-nano features. However, these technologies face many challenges when processing structures with smaller feature sizes. First, due to the limitations of machine tool accuracy and rigidity, it is difficult to ensure that the processed raised micro-nano features have extremely high dimensional accuracy and shape accuracy. Secondly, raised micro-nano features are easily affected by cutting forces and thermal stress factors during the processing, resulting in structural collapse and deformation problems, which seriously affect the processing quality. In addition, traditional processing technologies have low processing efficiency and high costs, and it is difficult to meet the needs of large-scale production.
[0004] In view of the above problems, it is necessary to optimize the existing micro-nano feature processing technology and combine a variety of advanced technical means such as nano-level polishing, photolithography, physical spraying and heat treatment to achieve high-precision, high-efficiency and low-roughness raised micro-nano feature processing. Therefore, the raised micro-nano feature processing process based on amorphous alloy proposed in the present invention is of great significance. Summary of the invention
[0005] The purpose of the present invention is to make up for the shortcomings of the prior art and provide a raised micro-nano feature processing technology based on amorphous alloys. It can ensure that the surface of the substrate is smooth and defect-free through nano-level polishing, and then use photolithography technology to form a precise pattern template on the substrate. On this basis, the amorphous alloy target is activated by a magnetron sputtering method and sprayed onto the substrate to form uniform raised micro-nano features only in the exposed area. Finally, the amorphous alloy is crystallized by heat treatment, which significantly enhances the bonding force between the coating and the substrate and prevents the collapse and deformation of the raised micro-nano features. It not only improves the processing accuracy and efficiency, but also reduces the production cost, providing a new solution for high-precision and high-efficiency processing of micro-nano devices.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a protruding micro-nano feature processing technology based on amorphous alloy, the specific steps of the process are:
[0007] S100, metal surface polishing: polish the surface of the metal base mold to the nanometer level;
[0008] S200, photoresist coating: coating a uniform layer of photoresist on the metal substrate by using a coating machine to form a photoresist layer;
[0009] S300, forming grooves by exposure technology: forming designed groove patterns on the surface of the photoresist by exposure technology, and these groove patterns will serve as templates for subsequent spraying of amorphous alloys;
[0010] S400, activation and spraying of amorphous alloy targets: Activate the amorphous alloy targets by magnetron sputtering, so that the exposed structures on the metal substrate are sprayed to form uniform raised micro-nano features;
[0011] S500, photoresist removal and post-processing: using toluene and propanol organic solvents to wash away the photoresist, exposing the complete raised micro-nano feature structure;
[0012] S600, quality inspection and evaluation: heat treatment of metal micro-nano devices to crystallize amorphous alloys, thereby improving the bonding strength between the coating and the substrate.
[0013] Furthermore, the S100 includes:
[0014] S101, cleaning treatment: select a metal base mold that meets the processing requirements and measure its initial surface roughness. Use an ultrasonic cleaning machine with deionized water and a special cleaning agent to thoroughly clean the mold surface to remove grease, dirt and impurities;
[0015] S102, rough polishing: mechanical polishing technology, using coarse-grained polishing liquid and polishing cloth, preliminary polishing of the mold surface to remove larger surface unevenness;
[0016] S103, fine polishing: Use fine-grained polishing liquid and softer polishing cloth to continue polishing the mold surface, gradually reducing the surface roughness to the nanometer level.
[0017] Furthermore, the S200 includes:
[0018] S201, parameter adjustment: placing the metal substrate mold in a glue-spinning machine, and adjusting the rotation speed and time of the glue-spinning machine;
[0019] S202, coating operation: drop the photoresist on the center of the metal substrate mold, start the coating machine, and evenly coat the photoresist on the substrate surface to form a uniform photoresist layer with controllable thickness;
[0020] S203, pre-baking treatment: placing the metal substrate mold coated with the photoresist in a drying oven, setting the temperature and time for pre-baking treatment.
[0021] Furthermore, the S300 includes:
[0022] S301, template selection: prepare a mask with a raised micro-nano structure pattern according to design requirements;
[0023] S302, exposure preparation: accurately align the mask plate above the metal base mold coated with photoresist, and adjust the light source parameters of the exposure machine;
[0024] S303, exposure operation: starting an exposure machine to irradiate light onto the photoresist layer through the mask plate, and forming a groove pattern corresponding to the mask plate pattern on the photoresist surface according to the photosensitivity characteristics of the photoresist;
[0025] S304, development treatment: using a specific developer to develop the exposed photoresist layer, remove the unexposed portion of the photoresist, and leave a photoresist structure corresponding to the groove pattern.
[0026] Furthermore, the specific steps of performing the development process in S304 are as follows:
[0027] (1) Gently spray a layer of deionized water on the surface of the substrate after photoresist coating and exposure;
[0028] (2) using a special developing nozzle to spray the developing solution on the substrate surface, controlling the flow rate and speed of the developing solution so that it evenly covers the photoresist surface;
[0029] (3) After spraying, the developer stays on the surface of the photoresist to allow the developer and the photoresist to fully react;
[0030] (4) Rinse the substrate surface with deionized water to remove residual developer and photoresist.
[0031] Furthermore, the S400 includes:
[0032] S401, activation treatment: select high-quality amorphous alloy target materials, and use magnetron sputtering method to activate the target materials so that the atoms or molecules on their surface are in a high-energy state;
[0033] S402, spraying operation: placing the activated amorphous alloy target in the spraying equipment, and by precisely controlling the spraying parameters, spraying the amorphous alloy material uniformly onto the exposed structural surface of the metal substrate to form uniform raised micro-nano features.
[0034] Furthermore, the specific steps of activating the target material by using the magnetron sputtering method in S401 are as follows:
[0035] (1) Select high-quality amorphous alloy target and install the target at the cathode position of the magnetron sputtering equipment;
[0036] (2) filling the chamber of the magnetron sputtering equipment with an inert gas to form a protective atmosphere and serve as a sputtering medium, and adjusting the gas pressure and temperature in the chamber;
[0037] (3) Apply a high voltage between the anode and cathode to generate an electric field, and set a magnetic field around the target to control the trajectory of electrons and the bombardment direction of Ar ions;
[0038] (4) Under the action of the electric field force, the electrons are accelerated in the chamber and collide with the argon atoms, generating Ar ion and electron avalanche effects. The Ar ions are accelerated and bombard the target surface, causing the atoms or molecules on the target surface to be sputtered out. The sputtered particles will collide with the gas molecules in the process of flying to the substrate and lose some energy, but most of the particles can still maintain a high energy state;
[0039] (5) High-energy particles, i.e., activated target particles, are guided and deposited on the substrate material under the action of the magnetic field to form a uniform thin film layer.
[0040] Furthermore, the S500 includes:
[0041] S501, photoresist removal: using toluene and propanol organic solvents, soaking, cleaning and rinsing the photoresist on the metal substrate to completely remove the residual photoresist;
[0042] S502, cleaning and drying: cleaning the metal substrate again with deionized water cleaning agent to remove the residual organic solvent, and thoroughly drying the substrate through a drying device;
[0043] S503, heating crystallization: placing the dried metal micro-nano device in a heating furnace for heating treatment, so that the amorphous alloy coating undergoes a crystallization reaction at high temperature, thereby improving the bonding strength between the coating and the substrate.
[0044] Furthermore, the specific steps of heating and crystallization in S503 are:
[0045] (1) placing the substrate sample coated with the amorphous alloy in a heating device, setting the heating temperature and heating rate, and starting the heating device;
[0046] (2) When the sample reaches the predetermined crystallization temperature, it enters the heat preservation stage. During the heat preservation process, the atoms in the amorphous alloy coating begin to rearrange to form an ordered crystal structure;
[0047] (3) After the insulation is completed, the sample is cooled and the cooling rate is controlled to obtain the desired crystallization effect. After the sample gradually cools to room temperature, it is taken out and subsequently processed and tested.
[0048] Furthermore, the S600 includes:
[0049] S601, appearance inspection: Use optical microscope and SEM tools to conduct appearance inspection on processed metal micro-nano devices to confirm whether the shape, size and distribution of raised micro-nano features meet the design requirements;
[0050] S602, performance test: Comprehensively evaluate the performance of metal micro-nano devices through mechanical testing, electrical performance testing, and thermal performance testing;
[0051] S603, Data Analysis and Summary: Collect and organize various data during the processing, including key indicators of surface roughness, coating thickness, and bonding strength, and conduct data analysis and summary to provide a basis for subsequent process optimization.
[0052] Compared with the prior art, this protruding micro-nano feature processing technology based on amorphous alloy has the following advantages:
[0053] Beneficial effects:
[0054] 1. The present invention adopts plasma beam and magnetron sputtering technology to effectively activate the amorphous alloy target material and realize uniform spraying on the metal substrate to form raised micro-nano features, which not only improves the bonding force between the amorphous alloy coating and the metal substrate, but also promotes the crystallization of the amorphous alloy through subsequent heating treatment, further enhances the hardness and wear resistance of the coating, prolongs the service life of the micro-nano device, and broadens its application field.
[0055] 2. The present invention successfully forms the raised micro-nano structure template required for the design on the metal substrate through metal surface polishing and photoresist coating technology, combined with high-precision exposure and development processing. The nanometer-level surface polishing ensures the flatness of the substrate and provides a high-quality substrate for subsequent processing. The uniform coating of the photoresist and the precise exposure and development ensure the accurate replication of the raised micro-nano structure, avoiding the errors and defects that may be caused by traditional processing methods.
[0056] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0058] Figure 1 The figure is an operation flow chart of a raised micro-nano feature processing technology based on amorphous alloys.
[0059] Figure 2 The figure is a process flow chart of a raised micro-nano feature processing technology based on amorphous alloys. DETAILED DESCRIPTION
[0060] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] Embodiment 1
[0062] A raised micro-nano feature processing technology based on amorphous alloys, the method comprises the following steps: metal surface polishing, photoresist coating, exposure technology to form grooves, activation and spraying of amorphous alloy targets, photoresist removal and post-processing, and quality inspection and evaluation.
[0063] First, enter the metal surface polishing stage (S100), select a suitable metal base mold, including stainless steel, nickel-based alloy, and thoroughly clean the surface to remove oil and oxide layer impurities, install the mold on a polishing machine, use coarse-grained diamond polishing liquid and a harder polishing cloth for preliminary polishing to remove obvious surface defects and unevenness, then replace it with fine-grained aluminum oxide polishing liquid and a softer polishing cloth, and continue polishing until the surface roughness reaches the nanometer level. Use an optical microscope or an atomic force microscope to check the polishing effect. After confirming that the surface is scratch-free and smooth, thoroughly clean the mold with deionized water and dry it.
[0064] Next, enter the photoresist coating stage (S200), select the appropriate photoresist type according to the process requirements, and ensure that it is within the specified service life, place the metal substrate mold in a coating machine, set the appropriate rotation speed and time, drop photoresist on the center of the mold, start the coating machine to spread the photoresist evenly, place the coated mold in a drying oven, set the appropriate temperature and time to remove the solvent in the photoresist and enhance its adhesion to the substrate.
[0065] Subsequently, the exposure technology is used to form grooves (S300). According to the design requirements, a mask with a raised micro-nano structure pattern is prepared, and the mask is precisely aligned above the metal base mold coated with photoresist. The light source parameters of the exposure machine are adjusted, and the exposure machine is started to allow light to pass through the mask and irradiate the photoresist layer. According to the photosensitivity of the photoresist, a groove pattern corresponding to the mask pattern is formed on the surface of the photoresist. A specific developer is used to develop the exposed photoresist layer to remove the unexposed part of the photoresist, leaving a photoresist structure corresponding to the groove pattern.
[0066] Then, the activation and spraying stage of the amorphous alloy target (S400) is entered, and a suitable amorphous alloy target, such as an iron-based, nickel-based or cobalt-based amorphous alloy, is selected, and necessary pretreatment is performed. The target is activated by a plasma beam or magnetron sputtering technology to make the amorphous alloy material in a state that is easy to spray. The spraying equipment is controlled to accurately spray the activated amorphous alloy material into the groove defined by the photoresist to form the desired micro-nano structure.
[0067] Next, enter the photoresist removal and post-processing stage (S500), use acetone, toluene or propanol organic solvent to soak or spray the mold to dissolve and remove the photoresist, pay attention to controlling the amount of solvent and soaking time to avoid damage to the micro-nano structure, thoroughly clean the mold with deionized water to remove residual solvent and impurities, and then dry it. Place the dried metal micro-nano device in a heating furnace for heating treatment to make the amorphous alloy coating crystallize at high temperature to improve the bonding strength between the coating and the substrate, and further clean, passivate or encapsulate as needed to improve the stability and durability of the micro-nano structure.
[0068] Finally, the quality inspection and evaluation stage (S600) is entered, and the morphology and dimensional accuracy of the micro-nano structure are observed using a scanning electron microscope (SEM), a transmission electron microscope (TEM) or an atomic force microscope (AFM), and the performance indicators of the micro-nano structure such as hardness, conductivity, and corrosion resistance are evaluated through mechanical testing, electrical testing, and chemical stability testing methods.
[0069] In summary, this embodiment achieves high-precision and high-efficiency processing of raised micro-nano features on a metal substrate through metal surface polishing, photoresist coating, exposure technology to form grooves, activation and spraying of amorphous alloy targets, removal and post-processing of photoresist, and quality inspection and evaluation steps, providing a new technical means for the field of micro-nano manufacturing.
[0070] Embodiment 2
[0071] Based on the first embodiment, this embodiment describes in detail an exposure technology for forming grooves based on amorphous alloy raised micro-nano feature processing technology, activation and spraying of amorphous alloy target materials, and removal and post-processing steps of photoresist.
[0072] In the groove forming stage of the exposure technology, a specific developer is used to develop the exposed photoresist layer, remove the unexposed part of the photoresist, and leave the photoresist structure corresponding to the groove pattern. The specific steps of the development process are:
[0073] (1) Gently spray a layer of deionized water on the surface of the substrate after photoresist coating and exposure;
[0074] (2) using a special developing nozzle to spray the developing solution on the substrate surface, controlling the flow rate and speed of the developing solution so that it evenly covers the photoresist surface;
[0075] (3) After spraying, the developer stays on the surface of the photoresist to allow the developer and the photoresist to fully react;
[0076] (4) Rinse the substrate surface with deionized water to remove residual developer and photoresist.
[0077] During the activation and spraying stage of the amorphous alloy target, a suitable amorphous alloy target, such as iron-based, nickel-based or cobalt-based amorphous alloy, is selected and necessary pretreatment is performed. The target is activated by magnetron sputtering technology to make the amorphous alloy material in a state that is easy to spray. The spraying equipment is controlled to accurately spray the activated amorphous alloy material into the groove defined by the photoresist to form the desired micro-nano structure.
[0078] The specific steps of activating the target material by magnetron sputtering technology to make the amorphous alloy material in a state that is easy to spray are:
[0079] (1) Select high-quality amorphous alloy target and install the target at the cathode position of the magnetron sputtering equipment;
[0080] (2) filling the chamber of the magnetron sputtering equipment with an inert gas to form a protective atmosphere and serve as a sputtering medium, and adjusting the gas pressure and temperature in the chamber;
[0081] (3) Apply a high voltage between the anode and cathode to generate an electric field, and set a magnetic field around the target to control the trajectory of electrons and the bombardment direction of Ar ions;
[0082] (4) Under the action of the electric field force, the electrons are accelerated in the chamber and collide with argon atoms, generating Ar ion and electron avalanche effects. The Ar ions are accelerated and bombard the surface of the target material, causing the atoms or molecules on the surface of the target material to be sputtered out. The sputtered particles will collide with gas molecules in the process of flying to the substrate and lose some energy, but most of the particles can still maintain a high energy state.
[0083] (5) High-energy particles, i.e., activated target particles, are guided and deposited on the substrate material under the action of the magnetic field to form a uniform thin film layer.
[0084] During the photoresist removal and post-processing stage, the mold is soaked or sprayed with toluene and propanol organic solvents to dissolve and remove the photoresist. Care is taken to control the amount of solvent and the soaking time to avoid damage to the micro-nano structure. The mold is thoroughly cleaned with deionized water to remove residual solvent and impurities, and then dried. The dried metal micro-nano device is placed in a heating furnace for heating treatment to allow the amorphous alloy coating to crystallize at high temperature, thereby increasing the bonding strength between the coating and the substrate. Further cleaning, passivation or packaging treatment is performed as needed to improve the stability and durability of the micro-nano structure.
[0085] The specific steps of the crystallization reaction are:
[0086] (1) placing the substrate sample coated with the amorphous alloy in a heating device, setting the heating temperature and heating rate, and starting the heating device;
[0087] (2) When the sample reaches the predetermined crystallization temperature, it enters the heat preservation stage. During the heat preservation process, the atoms in the amorphous alloy coating begin to rearrange to form an ordered crystal structure;
[0088] (3) After the insulation is completed, the sample is cooled and the cooling rate is controlled to obtain the desired crystallization effect. After the sample gradually cools to room temperature, it is taken out and subsequently processed and tested.
[0089] In summary, this embodiment forms a precise pattern template on the substrate by utilizing photolithography technology, activates the amorphous alloy target by using a magnetron sputtering method, sprays it onto the substrate, and crystallizes the amorphous alloy by heat treatment, thereby significantly enhancing the bonding force between the coating and the substrate and preventing the collapse and deformation of the raised micro-nano features.
[0090] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A protruding micro-nano feature processing technology based on amorphous alloy, characterized in that: The specific steps of this process are: S100, metal surface polishing: polish the surface of the metal base mold to the nanometer level; S200, photoresist coating: coating a uniform layer of photoresist on the metal substrate by using a coating machine to form a photoresist layer; S300, forming grooves by exposure technology: forming designed groove patterns on the surface of the photoresist by exposure technology, and these groove patterns will serve as templates for subsequent spraying of amorphous alloys; S400, activation and spraying of amorphous alloy targets: Activate the amorphous alloy targets by magnetron sputtering, so that the exposed structures on the metal substrate are sprayed to form uniform raised micro-nano features; S500, photoresist removal and post-processing: using toluene and propanol organic solvents to wash away the photoresist, exposing the complete raised micro-nano feature structure; S600, quality inspection and evaluation: heat treatment of metal micro-nano devices to crystallize amorphous alloys, thereby improving the bonding strength between the coating and the substrate.
2. According to the process for processing raised micro-nano features based on amorphous alloys as claimed in claim 1, it is characterized in that: The S100 includes: S101, cleaning treatment: select a metal base mold that meets the processing requirements and measure its initial surface roughness. Use an ultrasonic cleaning machine with deionized water and a special cleaning agent to thoroughly clean the mold surface to remove grease, dirt and impurities; S102, rough polishing: mechanical polishing technology, using coarse-grained polishing liquid and polishing cloth, preliminary polishing of the mold surface to remove larger surface unevenness; S103, fine polishing: Use fine-grained polishing liquid and softer polishing cloth to continue polishing the mold surface, gradually reducing the surface roughness to the nanometer level.
3. According to the process for processing raised micro-nano features based on amorphous alloys as claimed in claim 1, it is characterized in that: The S200 includes: S201, parameter adjustment: placing the metal substrate mold in a glue-spinning machine, and adjusting the rotation speed and time of the glue-spinning machine; S202, coating operation: drop the photoresist on the center of the metal substrate mold, start the coating machine, and evenly coat the photoresist on the substrate surface to form a uniform photoresist layer with controllable thickness; S203, pre-baking treatment: placing the metal substrate mold coated with the photoresist in a drying oven, setting the temperature and time for pre-baking treatment.
4. The process for processing raised micro-nano features based on amorphous alloys according to claim 1, characterized in that: The S300 includes: S301, template selection: prepare a mask with a raised micro-nano structure pattern according to design requirements; S302, exposure preparation: accurately align the mask plate above the metal base mold coated with photoresist, and adjust the light source parameters of the exposure machine; S303, exposure operation: starting an exposure machine to irradiate light onto the photoresist layer through the mask plate, and forming a groove pattern corresponding to the mask plate pattern on the photoresist surface according to the photosensitivity characteristics of the photoresist; S304, development treatment: using a specific developer to develop the exposed photoresist layer, remove the unexposed portion of the photoresist, and leave a photoresist structure corresponding to the groove pattern.
5. A protruding micro-nano feature processing technology based on amorphous alloy according to claim 4, characterized in that: The specific steps of performing the development process in S304 are as follows: (1) Gently spray a layer of deionized water on the surface of the substrate after photoresist coating and exposure; (2) using a special developing nozzle to spray the developing solution on the substrate surface, controlling the flow rate and speed of the developing solution so that it evenly covers the photoresist surface; (3) After spraying, the developer stays on the surface of the photoresist to allow the developer and the photoresist to fully react; (4) Rinse the substrate surface with deionized water to remove residual developer and photoresist.
6. The process for processing raised micro-nano features based on amorphous alloys according to claim 4, characterized in that: The S400 includes: S401, activation treatment: select high-quality amorphous alloy target materials, and use magnetron sputtering method to activate the target materials so that the atoms or molecules on their surface are in a high-energy state; S402, spraying operation: placing the activated amorphous alloy target in the spraying equipment, and by precisely controlling the spraying parameters, spraying the amorphous alloy material uniformly onto the exposed structural surface of the metal substrate to form uniform raised micro-nano features.
7. The process for processing raised micro-nano features based on amorphous alloys according to claim 1, characterized in that: The specific steps of activating the target material by using the magnetron sputtering method in S401 are as follows: (1) Select high-quality amorphous alloy target and install the target at the cathode position of the magnetron sputtering equipment; (2) filling the chamber of the magnetron sputtering equipment with an inert gas to form a protective atmosphere and serve as a sputtering medium, and adjusting the gas pressure and temperature in the chamber; (3) Apply a high voltage between the anode and cathode to generate an electric field, and set a magnetic field around the target to control the trajectory of electrons and the bombardment direction of Ar ions; (4) Under the action of the electric field force, the electrons are accelerated in the chamber and collide with the argon atoms, generating Ar ion and electron avalanche effects. The Ar ions are accelerated and bombard the target surface, causing the atoms or molecules on the target surface to be sputtered out. The sputtered particles will collide with the gas molecules in the process of flying to the substrate and lose some energy, but most of the particles can still maintain a high energy state; (5) High-energy particles, i.e., activated target particles, are guided and deposited on the substrate material under the action of the magnetic field to form a uniform thin film layer.
8. The process for processing raised micro-nano features based on amorphous alloys according to claim 1, characterized in that: The S500 includes: S501, photoresist removal: using toluene and propanol organic solvents, soaking, cleaning and rinsing the photoresist on the metal substrate to completely remove the residual photoresist; S502, cleaning and drying: cleaning the metal substrate again with deionized water cleaning agent to remove the residual organic solvent, and thoroughly drying the substrate through a drying device; S503, heating and crystallization: placing the dried metal micro-nano device in a heating furnace for heating treatment to cause the amorphous alloy coating to undergo a crystallization reaction at a high temperature.
9. The process for processing raised micro-nano features based on amorphous alloys according to claim 1, characterized in that: The specific steps of heating and crystallization in S503 are: (1) placing the substrate sample coated with the amorphous alloy in a heating device, setting the heating temperature and heating rate, and starting the heating device; (2) When the sample reaches the predetermined crystallization temperature, it enters the heat preservation stage. During the heat preservation process, the atoms in the amorphous alloy coating begin to rearrange to form an ordered crystal structure; (3) After the insulation is completed, the sample is cooled and the cooling rate is controlled to obtain the desired crystallization effect. After the sample gradually cools to room temperature, it is taken out and subsequently processed and tested.
10. The process for processing raised micro-nano features based on amorphous alloys according to claim 1, characterized in that: The S600 includes: S601, appearance inspection: Use optical microscope and SEM tools to conduct appearance inspection on processed metal micro-nano devices to confirm whether the shape, size and distribution of raised micro-nano features meet the design requirements; S602, performance test: Comprehensively evaluate the performance of metal micro-nano devices through mechanical testing, electrical performance testing, and thermal performance testing; S603, Data Analysis and Summary: Collect and organize various data during the processing, including key indicators of surface roughness, coating thickness, and bonding strength, and conduct data analysis and summary to provide a basis for subsequent process optimization.
Citation Information
Cited By
Cross-band multistage adjustable radar wave-absorbing structure, design method and preparation method
CN121663214A