Bonding method, bonding structure, MEMS device and manufacturing method thereof

By using the top metal stack of the aluminum-titanium-aluminum sandwich structure in the aluminum-germanium eutectic bonding process of the MEMS gyroscope, the diffusion of the germanium layer and the bottom aluminum layer is blocked to form a thinner and consistent aluminum-germanium interfusion bonding The layer solves the problems of poor bond consistency and overflow, and improves the yield and performance of the device.

CN118929569APending Publication Date: 2024-11-12NINGBO SEMICON INT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536946.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing aluminum-germanium eutectic bonding process has poor bonding consistency on the entire wafer, resulting in a degradation of the performance of the MEMS gyroscope. If the bonding is too thin or too thick, it may cause the circuit to be shorted, affecting the device yield.

Method used

A patterned germanium layer is formed on the surface of the first substrate, and a top metal stack of aluminum-titanium-aluminum sandwich structure is formed on the surface of the second substrate. By blocking the mutual diffusion of the germanium layer and the bottom aluminum layer, only the The top aluminum layer is bonded to the germanium layer to form a thinner and consistent aluminum-germanium interfusion bonding layer.

Benefits of technology

It improves the thickness consistency of the aluminum-germanium bonding layer, reduces the possibility of overflow during bonding, avoids circuit shorting, and improves the yield and performance stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929569A_ABST
    Figure CN118929569A_ABST
Patent Text Reader

Abstract

The invention discloses a bonding method, a bonding structure, an MEMS device and a manufacturing method thereof. The bonding method comprises the following steps: providing a first substrate; forming a patterned germanium layer on the front surface of the first substrate; providing a second substrate; forming a patterned top metal lamination layer on the front surface of the second substrate, wherein the top metal lamination layer comprises a first aluminum layer located on the second substrate, a diffusion barrier layer located on the first aluminum layer and a second aluminum layer located on the diffusion barrier layer; aligning the germanium layer on the front surface of the first substrate with the top metal layer on the front surface of the second substrate; and bonding the second aluminum layer and the germanium layer together to form an aluminum-germanium mutual fusion bonding layer. According to the invention, the consistency of aluminum-germanium bonding can be improved, so that the performance of the MEMS device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor device manufacturing, and in particular to a bonding method, a bonding structure, a MEMS device and a manufacturing method thereof. Background Art

[0002] MEMS (micro-electro-mechanical system) gyroscopes are very susceptible to dust, water vapor, mechanical factors and other factors during the dicing and packaging process due to their movable microstructures, which can cause device damage or device performance degradation. Therefore, MEMS gyroscopes require airtight packaging to prevent damage to the movable microstructure, and at the same time maintain a stable gas damping coefficient to improve device performance.

[0003] Eutectic bonding is a wafer-level vacuum packaging technology that has been widely used in sensors such as accelerometers, gyroscopes, and pressure gauges in recent years, and has become a key technology for the development and practical application of MEMS devices. Eutectic bonding uses a metal layer as the intermediate bonding medium layer, taking advantage of the low melting temperature of some eutectic alloys, and heats and melts the two metals to tightly combine together to achieve bonding. Compared with other bonding methods commonly used in MEMS devices (anodic bonding, silicon-silicon direct bonding, and adhesive bonding), due to the use of metal dielectric materials, eutectic bonding sheets have lower permeability, so they can provide better airtightness levels. At the same time, the sealing metal ring required for eutectic bonding is narrower, so that new MEMS devices can meet smaller packaging size requirements. While forming a sealing metal ring, the eutectic bonding technology also provides an electrical path for the chip, which can easily introduce a vertical interconnected metal layer to realize wafer stacking packaging technology, thereby further reducing chip manufacturing and packaging costs.

[0004] The aluminum-germanium eutectic bonding process is often used in the production of MEMS gyroscopes. The principle of aluminum-germanium eutectic bonding is: by sputtering or evaporating aluminum-germanium metal layers of a certain thickness ratio on the surfaces of the two silicon wafers to be bonded, the aluminum-germanium metals melt and contact each other at a lower temperature. After mutual diffusion, an aluminum-germanium liquid alloy with a eutectic component is formed. As the diffusion time increases, the liquid alloy layer continues to thicken. After cooling, the aluminum-germanium metal in the liquid alloy layer grows based on its original solid phase, and the two metals are continuously and alternately precipitated to form a more stable crystal structure, thereby achieving bonding.

[0005] However, affected by the bonding machine, the current aluminum-germanium eutectic bonding process has poor bonding consistency. The total thickness of the AL / Ge bond varies in different areas of the entire wafer, affecting device performance. In addition, when the total thickness of the AL / Ge bond is too thin, that is, in an over-bonded state, the overflow of the AL / Ge in a molten state will cause a circuit short, resulting in device failure and affecting device yield. Summary of the invention

[0006] The object of the present invention is to provide a bonding method, a bonding structure, a MEMS device and a manufacturing method thereof, which can improve the consistency of aluminum-germanium bonding and thus improve the performance of the MEMS device.

[0007] To achieve the above object, in a first aspect, the present invention provides a bonding method, comprising:

[0008] providing a first substrate;

[0009] forming a patterned germanium layer on the front side of the first substrate;

[0010] providing a second substrate;

[0011] forming a patterned top metal stack on the front side of the second substrate, the top metal stack comprising a first aluminum layer on the second substrate, a diffusion barrier layer on the first aluminum layer, and a second aluminum layer on the diffusion barrier layer;

[0012] aligning the germanium layer on the front side of the first substrate with the top metal layer on the front side of the second substrate;

[0013] The second aluminum layer and the germanium layer are bonded together to form an aluminum-germanium mutual melting bonding layer.

[0014] In a second aspect, the present invention provides a bonding structure, comprising:

[0015] a first substrate;

[0016] A second substrate is located below the first substrate, and a top surface of the second substrate is bonded to a bottom surface of the first substrate via a metal bonding structure;

[0017] The metal bonding structure includes a patterned first aluminum layer located on the top surface of the second substrate, a diffusion barrier layer located on the first aluminum layer, and an aluminum-germanium mutual melting bonding layer located between the diffusion barrier layer and the first substrate;

[0018] The aluminum-germanium mutual melting bonding layer is formed by mutual melting of a patterned germanium layer located on the bottom surface of the first substrate and a second aluminum layer located on the diffusion barrier layer.

[0019] In a third aspect, the present invention provides a method for manufacturing a MEMS device, comprising:

[0020] Providing a cap wafer, wherein a plurality of openings are formed on the front side of the cap wafer;

[0021] Providing a device wafer, bonding the front side of the device wafer to the front side of the cap wafer, wherein the device wafer closes the opening to form a cavity;

[0022] Etching the back side of the device wafer to form a boss structure on the back side of the device wafer, wherein the boss structure is located at an edge region of the cavity;

[0023] forming a germanium layer on the top surface of the boss structure;

[0024] forming an interdigitated electrode structure in the device wafer, wherein the interdigitated electrode structure is located above the cavity;

[0025] Providing a base wafer, wherein an insulating layer is formed on the front side of the base wafer, and a wiring layer is formed in the insulating layer;

[0026] Forming a patterned top metal stack on the insulating layer, the top metal stack is electrically connected to the wiring layer, the top metal stack comprising a first aluminum layer located on the surface of the insulating layer, a diffusion barrier layer located on the first aluminum layer, and a second aluminum layer located on the diffusion barrier layer;

[0027] aligning the boss structure on the back side of the device wafer with the top metal stack on the substrate wafer;

[0028] The second aluminum layer and the germanium layer are bonded together to form an aluminum-germanium mutual melting bonding layer.

[0029] In a fourth aspect, the present invention provides a MEMS device, comprising:

[0030] A cap wafer, wherein the bottom surface of the cap wafer has a plurality of openings;

[0031] A device wafer is located below the cap wafer, the top surface of the device wafer is bonded to the bottom surface of the cap wafer, and the device wafer closes the opening to form a cavity;

[0032] The bottom surface of the device wafer has a boss structure, and the boss structure is located in the edge area of ​​the cavity; the device wafer has an interdigitated electrode structure, and the interdigitated electrode structure is located below the cavity;

[0033] A base wafer is located below the device wafer, the top surface of the base wafer has an insulating layer, and the insulating layer has a wiring layer;

[0034] The top surface of the base wafer and the boss structure on the bottom surface of the device wafer are bonded together via a metal bonding structure;

[0035] The metal bonding structure comprises a patterned first aluminum layer located on the surface of the insulating layer, a diffusion barrier layer located on the first aluminum layer, and an aluminum-germanium mutual melting bonding layer located between the diffusion barrier layer and the boss structure, wherein the first aluminum layer is electrically connected to the wiring layer;

[0036] The aluminum-germanium mutual melting bonding layer is formed by mutual melting of a germanium layer located on the surface of the boss structure and a second aluminum layer located on the diffusion barrier layer.

[0037] The beneficial effects of the present invention are:

[0038] The bonding method of the present invention forms a patterned germanium layer on the surface of the first substrate, and forms a top metal stack on the surface of the second substrate, wherein the top metal stack is formed by a first aluminum layer, a diffusion barrier layer, and a second aluminum layer. When the first substrate and the second substrate are bonded, the germanium layer on the first substrate is bonded to the second aluminum layer on the second substrate. Compared with the method of directly bonding the aluminum layer and the germanium layer in the prior art, the metal bonding layer on the second substrate in the present method is composed of a bottom aluminum layer-a diffusion barrier layer-a top aluminum layer. When the two substrates are bonded, the diffusion barrier layer can block the mutual diffusion between the metal germanium layer and the first aluminum layer at the bottom, that is, only the second aluminum layer at the top completes the bonding with the germanium layer. Since the thickness of the second aluminum layer can be thinner, the second aluminum layer The total thickness of the AL / Ge bonding layer formed after the second aluminum layer and the germanium layer are bonded is thinner, and thus the thickness difference of the AL / Ge mutual melting bonding layer in different areas on the bonding substrate is smaller, which can effectively improve the consistency of the thickness of the AL / Ge mutual melting bonding layer in different areas on the wafer; at the same time, during the bonding process, since the diffusion barrier layer located under the second aluminum layer can block the mutual diffusion between the metal germanium layer and the first aluminum layer at the bottom, the AL / Ge mutual melting bonding layer can achieve the effect of AL / Ge stratification; further, since the thickness of the second aluminum layer is thinner, the volume of the AL / Ge bonding is smaller, which can effectively avoid the problem of circuit short-circuit caused by AL / Ge mutual melting overflow during bonding, resulting in device function failure, thereby improving the yield of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figures 1 to 3 The device structure schematic diagram corresponding to each step of the existing MEMS gyroscope device manufacturing method is shown.

[0041] Figures 4 to 6 A schematic diagram of the device structure corresponding to each step in a bonding method according to embodiment 1 of the present invention is shown.

[0042] Figures 7 to 18 A schematic diagram of the device structure corresponding to each step in a method for manufacturing a MEMS device according to embodiment 3 of the present invention is shown. DETAILED DESCRIPTION

[0043] The existing manufacturing process of MEMS gyroscope is as follows: Figure 1-Figure 3 As shown, first, a cap wafer is provided, the cap wafer has an opening, an oxide layer is deposited on the surface of the cap wafer, a device wafer is bonded to the cap wafer, a cavity is formed between the device wafer and the cap wafer, and the structure after bonding is as shown in FIG. Figure 1 As shown; then the top surface of the device wafer is thinned, a boss structure is etched on the top surface of the device wafer, and then a germanium layer of a certain thickness is formed on the boss through deposition and patterning processes, and then the device wafer above the cavity is etched to form an interdigitated electrode structure. The structure formed is as shown Figure 2 After that, the structure is flipped over and the germanium layer on the boss is bonded to the aluminum layer on the top surface of the substrate wafer. The device structure is as shown in FIG. Figure 3 shown.

[0044] The above-mentioned aluminum-germanium eutectic bonding process is affected by the bonding machine, and the total thickness of AL / Ge bonding varies in different areas on the entire wafer. In some areas, AL / Ge over-bonding may occur, resulting in the total thickness of AL / Ge melt being too thin, and the distance (h) from the end of the fork finger to the top metal on the base wafer is affected by the bonding thickness, so capacitance and frequency failures may occur. At the same time, when the total thickness of AL / Ge bonding is too thin, the overflow of AL / Ge in a molten state may cause a circuit short circuit, resulting in failure.

[0045] To solve the above problems, the present invention provides a bonding method, a bonding structure, a MEMS device and a manufacturing method thereof, which can improve the control of aluminum-germanium bonding consistency, and is beneficial to improving device yield and bonding process control.

[0046] The following is a further detailed description of a bonding method, bonding structure, MEMS device and its manufacturing method of the present invention in combination with the accompanying drawings and specific embodiments. According to the following description and drawings, the advantages and features of the present invention will be clearer. However, it should be noted that the concept of the technical solution of the present invention can be implemented in a variety of different forms and is not limited to the specific embodiments described herein. The drawings are all in a very simplified form and are not in precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0047] The terms "first", "second", "upper", "lower", "top surface", "bottom surface", etc. in the specification and claims are used to distinguish between similar elements and are not necessarily used to describe a specific order, a temporal sequence or a specific spatial position. It is to be understood that, where appropriate, these terms used in this way are interchangeable, for example, so that the embodiments of the present invention described herein can be operated in an order other than that described or shown herein. Similarly, if the method described herein includes a series of steps, the order of these steps presented herein is not necessarily the only order in which these steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method. If the components in a certain figure are the same as the components in other figures, although these components can be easily identified in all figures, in order to make the description of the figures clearer, this specification will not mark all the same component numbers in each figure.

[0048] Example 1

[0049] like Figure 4-Figure 6 As shown, this embodiment provides a bonding method, including:

[0050] like Figure 4 As shown, a first substrate 100 is provided; a patterned germanium layer 105 is formed on the front side of the first substrate 100;

[0051] A germanium layer 105 can be formed on the front side of the first substrate 100 by physical vapor deposition or chemical vapor deposition methods such as magnetron sputtering and evaporation, and then the germanium layer 105 is patterned by a patterning process. The patterned germanium layer 105 serves as a metal bonding layer, and its shape is not limited, and it can be annular, circular, rectangular, etc., which can be selected according to the specific bonding requirements of the device.

[0052] like Figure 5 As shown, a second substrate 200 is provided;

[0053] forming a patterned top metal stack on the front side of the second substrate 200, wherein the top metal stack comprises a first aluminum layer 112 located on the second substrate 200, a diffusion barrier layer 113 located on the first aluminum layer 112, and a second aluminum layer 114 located on the diffusion barrier layer 113;

[0054] Preferably, the material of the diffusion barrier layer 113 is titanium.

[0055] The method for forming the top metal layer comprises:

[0056] Forming a first aluminum layer 112 on the surface of the second substrate 200 and patterning the first aluminum layer 112;

[0057] forming a titanium layer to cover the surface of the patterned first aluminum layer 112 and the exposed surface of the second substrate 200;

[0058] Patterning the titanium layer to remove the titanium layer on the surface of the second substrate 200;

[0059] forming a second aluminum layer 114 to cover the surface of the patterned titanium layer and the exposed surface of the second substrate 200;

[0060] Patterning the second aluminum layer 114 and removing the second aluminum layer 114 on the surface of the second substrate 200;

[0061] Finally, a top metal stack structure of an aluminum-titanium-aluminum sandwich structure is formed, wherein the second aluminum layer 114 at the top layer serves as a metal bonding layer, and the diffusion barrier layer 113 (titanium layer) is used to block the aluminum-germanium mutual diffusion between the germanium layer 105 and the second aluminum layer 114 during aluminum-germanium eutectic bonding.

[0062] Preferably, the thickness of the top metal stack is The thickness of the second aluminum layer 114 located at the top layer is The thickness of the germanium layer 105 is preferably not less than the thickness of the second aluminum layer 114. The thickness ratio of the germanium layer 105 to the second aluminum layer 114 can be selected according to the process requirements. Optionally, the thickness range of the titanium layer is The thickness of the first aluminum layer 112 is in the range of

[0063] like Figure 6 As shown, the germanium layer 105 on the front side of the first substrate 100 is aligned with the top metal layer on the front side of the second substrate 200;

[0064] The second aluminum layer 114 and the germanium layer 105 are bonded together to form an aluminum-germanium inter-melting bonding layer 115. Preferably, the thickness of the second aluminum layer after bonding is The diffusion barrier layer 113 can prevent mutual diffusion between the germanium layer 105 and the first aluminum layer 112 during the bonding process.

[0065] The bonding of the second aluminum layer 114 and the germanium layer 105 is completed by a eutectic bonding process, and the specific method is as follows:

[0066] The patterns of the germanium layer 105 on the first substrate 100 and the top metal stack on the second substrate 200 are aligned and contacted, and then the first substrate 100 and the second substrate 200 are pressurized and heated for a set time, so that the metal germanium in the germanium layer 105 and the aluminum in the second aluminum layer 114 melt and diffuse with each other to form a liquid alloy layer, and then cool to form a stable aluminum-germanium metal bonding layer; preferably, the process conditions adopted in the eutectic bonding process include: bonding temperature: 400-500°C; bonding time: 5-15min; bonding pressure: 5000-7000mpa.

[0067] Compared with the existing method of directly eutectic bonding the thicker aluminum layer and the germanium layer 105, the top metal stack formed on the second substrate 200 in the present method adopts an aluminum-titanium-aluminum sandwich structure. Since metal titanium cannot eutectically react with metal aluminum or germanium, the titanium layer can effectively block the germanium layer 105 from diffusing toward the second aluminum layer 114 located at the bottom layer, thereby realizing the diffusion barrier effect between germanium and the first aluminum layer 112 at the bottom layer. Therefore, only the second aluminum layer 114 located at the top layer participates in the bonding. Since the second aluminum layer 114 is thinner, the titanium layer located between the first aluminum layer 112 and the second aluminum layer 114 during the bonding process can act as a diffusion barrier layer 113 to block the molten metal germanium from diffusing toward the first aluminum layer 112 located at the bottom layer, thereby preventing the finally formed aluminum-germanium intermelting bonding layer 115 from being too thick. At the same time, due to the presence of the titanium layer, the stratification of aluminum-germanium in the metal bonding structure formed by the germanium layer 105 and the top metal stack is more obvious, thereby effectively controlling the thickness consistency of the aluminum-germanium intermelting bonding layer 115 in different regions on the wafer. In addition, the second aluminum layer 114 involved in eutectic bonding is thinner, and the overflow of molten aluminum germanium metal during the bonding process is less, which can avoid the short circuit problem caused by excessive overflow of molten metal on the circuit, thus avoiding device failure and improving yield.

[0068] It should be noted that the method of this embodiment can be applied to the preparation of any semiconducting device that requires an aluminum-germanium bonding process. Therefore, this embodiment does not limit the types of the first substrate 100 and the second substrate 200. The first substrate 100 and the second substrate 200 can be any suitable substrate known to those skilled in the art, for example, at least one of the following materials: silicon (Si), germanium (Ge), silicon germanium (SiGe), carbon silicon (SiC), carbon germanium silicon (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP) or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), or double-sided polished silicon wafers (Double Side Polished Wafers, DSP), or ceramic substrates such as aluminum oxide, quartz or glass substrates, etc. The first substrate 100 may have device structures such as cavities and functional devices, and the second substrate 200 may also have semiconductor device structures such as wiring layers and electrical connection structures.

[0069] Example 2

[0070] like Figure 6 As shown, this embodiment provides a bonding structure, which can be formed by the bonding method of embodiment 1, and the bonding structure includes:

[0071] A first substrate 100;

[0072] A second substrate 200 is located below the first substrate 100, and a top surface of the second substrate 200 is bonded to a bottom surface of the first substrate 100 via a metal bonding structure;

[0073] The metal bonding structure includes a patterned first aluminum layer 112 located on the top surface of the second substrate, a diffusion barrier layer 113 located on the first aluminum layer 112, and an aluminum-germanium mutual melting bonding layer 115 located between the diffusion barrier layer 113 and the first substrate 100;

[0074] refer to Figure 4-Figure 6 The aluminum-germanium mutual melting bonding layer 115 is formed by mutual melting of the patterned germanium layer 105 located on the bottom surface of the first substrate 100 and the second aluminum layer 114 located on the diffusion barrier layer 113 .

[0075] Preferably, the material of the diffusion barrier layer 113 is titanium; the thickness of the second aluminum layer before bonding is preferably The sum of the thicknesses of the first aluminum layer 112, the diffusion barrier layer 113 and the second aluminum layer 114 is The thickness of the germanium layer 105 is not less than the thickness of the second aluminum layer 114. The thickness ratio of the germanium layer to the second aluminum layer 114 can be selected according to the process requirements. The thickness range of the titanium layer is The thickness of the first aluminum layer 112 is in the range of The thickness of the second aluminum layer in the metal bonding structure (i.e. after bonding) is preferably

[0076] In the bonding structure of this embodiment, the top metal stack on the second substrate 200 adopts an aluminum-titanium-aluminum sandwich structure. Since metal titanium cannot react with metal aluminum or germanium eutectic, the titanium layer can effectively block the germanium layer 105 from diffusing to the second aluminum layer 114 located at the bottom during the eutectic bonding process, thereby achieving a diffusion barrier between germanium and the bottom aluminum. Therefore, during the bonding process, only the second aluminum layer 114 located at the top of the top metal stack is used to bond with the germanium layer 105 on the first substrate 100 to form the metal bonding structure. Since the second aluminum layer 114 is thinner, only Therefore, the thickness of the aluminum-germanium intermelting bonding layer 115 finally formed is thinner, which can be more conducive to controlling the thickness consistency of the aluminum-germanium intermelting bonding layer 115 in different areas on the chip, and it is less likely to produce excessive metal overflow during the bonding process, which can avoid problems such as circuit short circuit caused by overflow, and the device function is less likely to fail, and the yield is higher.

[0077] Example 3

[0078] like Figure 7-Figure 18 As shown, this embodiment provides a method for manufacturing a MEMS device, comprising:

[0079] like Figure 7 As shown, a cap wafer 101 is provided, and a plurality of openings are formed on the front side of the cap wafer 101;

[0080] The material of the cap wafer 101 refers to the material of the first substrate 100 or the second substrate 200 in Example 1. The material of the cap wafer 101 of this embodiment is single crystal silicon. The opening on the front of the cap wafer 101 can be formed by an etching process, and the shape of the bottom surface of the opening is preferably rectangular. A dielectric layer 102 is also formed on the front of the cap wafer 101. The material of the dielectric layer 102 can be any suitable dielectric material, including but not limited to at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride and the like. The dielectric layer 102 can be formed by depositing silicon oxide.

[0081] like Figure 8As shown, a device wafer 103 is provided, and the front side of the device wafer 103 is bonded to the front side of the cap wafer 101 . The device wafer 103 closes the opening to form a cavity; the cavity is used to form a working space for the subsequently formed interdigitated electrode structure 107 .

[0082] The device wafer 103 is used as a device structure layer for subsequently forming a boss structure 104 and an interdigitated electrode structure 107 . In this embodiment, the material of the device wafer 103 is preferably single crystal silicon.

[0083] like Fig. 9 As shown, the back side of the device wafer 103 is thinned, and then the back side of the device wafer 103 is etched to form a boss structure 104 on the back side of the device wafer 103, and the boss structure 104 is located at the edge area of ​​the cavity;

[0084] The etching process for forming the boss structure 104 can be a wet etching process or a dry etching process, wherein a dry etching process is preferably used, and dry etching includes but is not limited to reactive ion etching (RIE), ion beam etching, plasma etching or laser cutting. The dry etching can be, for example, inductively coupled plasma (ICP) etching, reactive ion etching (RIE), etc. The top surface of the boss structure 104 serves as a bonding surface, and the height of the boss structure 104 can be set according to the capacitance value required between the interdigitated electrode and the top metal on the base wafer 108.

[0085] like Fig.10 As shown, a germanium layer 105 is formed on the top surface of the boss structure 104;

[0086] The method of forming the germanium layer 105 includes:

[0087] A germanium layer 105 covering the convex platform structure 104 and the surface of the device wafer 103 is formed on the back side of the device wafer 103, and then the germanium layer 105 is patterned to retain only the germanium layer 105 on the top surface of the convex structure. The germanium layer 105 can be formed by a physical vapor deposition method such as magnetron sputtering or evaporation, or a chemical vapor deposition method. The thickness of the germanium layer 105 is not less than the thickness of the second aluminum layer 114 formed subsequently.

[0088] like Fig.11 As shown, an interdigitated electrode structure 107 is formed in the device wafer 103, and the interdigitated electrode structure 107 is located above the cavity;

[0089] The device wafer 103 above the cavity can be etched by an etching process to form an interdigitated electrode structure 107, and the gaps between the interdigitated fingers in the interdigitated electrode structure 107 are connected to the cavity. The etching process preferably adopts a dry etching process.

[0090] like Figure 12-14As shown, a base wafer 108 is provided, an insulating layer is formed on the front side of the base wafer 108, and a wiring layer 110 is formed in the insulating layer;

[0091] The material of the base wafer 108 refers to the material of the first substrate 100 in Example 1. <100> P-type high-resistance single-crystal silicon wafer with different crystal orientations.

[0092] The method for forming the insulating layer and the wiring layer 110 on the base wafer 108 includes:

[0093] like Fig.12 As shown, a first insulating layer 109 is formed on a base wafer 108, and then the first insulating layer 109 is patterned;

[0094] like Fig.13 As shown, a conductive metal layer is formed on the first insulating line, and then the conductive metal layer is patterned to form a wiring layer 110.

[0095] like Fig.14 As shown, a second insulating layer 111 is formed on the wiring layer 110, and then the second insulating layer 111 is patterned to expose the underlying wiring layer 110.

[0096] The first insulating layer 109 and the second insulating layer 111 together constitute the insulating layer. The first insulating layer 109 and the second insulating layer 111 are made of the same material, which can be any suitable dielectric material, including but not limited to at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, etc. In this embodiment, it is silicon oxide. The material of the wiring layer 110 can be any conductive metal material, such as copper, aluminum, gold, silver, etc. In this embodiment, the material of the wiring layer 110 is aluminum. The thickness of the wiring layer 110 is preferably The first insulating layer 109 and the second insulating layer 111 can be formed by any suitable deposition method known to those skilled in the art, such as chemical vapor deposition, physical vapor deposition or atomic layer deposition. The wiring layer 110 can be formed by physical vapor deposition or chemical vapor deposition methods such as magnetron sputtering and evaporation.

[0097] like Figure 15-17 As shown, a patterned top metal stack is formed on the insulating layer, the top metal stack is electrically connected to the wiring layer 110, and the top metal stack includes a first aluminum layer 112 located on the surface of the insulating layer, a diffusion barrier layer 113 located on the first aluminum layer 112, and a second aluminum layer 114 located on the diffusion barrier layer 113; preferably, the material of the diffusion barrier layer 113 is titanium.

[0098] The method of forming a patterned top metal stack on the insulating layer comprises:

[0099] like Fig.15As shown, firstly, a first aluminum layer 112 is formed on the second insulating layer 111, the first aluminum layer 112 is electrically connected to the wiring layer 110, and then the first aluminum layer 112 is patterned by an etching process;

[0100] like Fig.16 As shown, a diffusion barrier layer 113, i.e., a titanium layer, is then formed to cover the surfaces of the first aluminum layer 112 and the second insulating layer 111. The titanium layer on the surface of the second insulating layer 111 is removed by a patterning process, and the titanium layer on the surface of the first aluminum layer 112 is retained;

[0101] like Fig.17 As shown, a second aluminum layer 114 is then formed covering the surface of the titanium layer and the surface of the second insulating layer 111. The second aluminum layer 114 on the surface of the second insulating layer 111 is removed by a graphical process, and the second aluminum layer 114 on the surface of the titanium layer is retained, thereby finally forming a top metal stack of an aluminum-germanium-aluminum sandwich structure.

[0102] The first aluminum layer 112, the titanium layer and the second aluminum layer 114 can be formed by physical vapor deposition or chemical vapor deposition methods such as magnetron sputtering and evaporation. Preferably, the thickness of the top metal stack is The thickness of the second aluminum layer 114 located at the top layer is The thickness ratio of the germanium layer 105 to the second aluminum layer 114 can be selected according to the process requirements; the thickness range of the titanium layer is The thickness of the first aluminum layer 112 is in the range of

[0103] like Fig.18 As shown, the boss structure 104 on the back side of the device wafer 103 is aligned with the top metal stack on the substrate wafer;

[0104] The second aluminum layer 114 and the germanium layer 105 are bonded together to form an aluminum-germanium mutual melting bonding layer 115. The thickness of the second aluminum layer 114 after bonding is The diffusion barrier layer 113 can prevent mutual diffusion between the germanium layer 105 and the first aluminum layer 112 during the bonding process.

[0105] The MEMS device finally formed in this embodiment is a gyroscope, in which the bonding of the second aluminum layer 114 and the germanium layer 105 is completed by a eutectic bonding process, and the specific method is:

[0106] The back side of the device wafer 103 is placed opposite to the front side of the base wafer 108, and the boss structure 104 is aligned with the pattern of the top metal stack, so that the germanium layer 105 on the boss structure 104 is in contact with the second aluminum layer 114, and then the cap wafer 101 / device wafer 103 and the base wafer 108 are pressurized and heated for a set time, so that the metal germanium in the germanium layer 105 and the aluminum in the second aluminum layer 114 melt and diffuse with each other to form a liquid alloy layer, and then a stable aluminum-germanium metal bonding layer is formed after cooling; preferably, the process conditions adopted in the eutectic bonding process include: bonding temperature: 400-500°C; bonding time: 5-15min; bonding pressure: 5000-7000mpa.

[0107] Compared with the existing method of directly eutectic bonding the thicker aluminum layer and the germanium layer 105, the top metal stack formed on the base wafer 108 in this method adopts an aluminum-titanium-aluminum sandwich structure. Since metal titanium cannot eutectically react with metal aluminum or germanium, the titanium layer can effectively block the germanium layer 105 from diffusing to the second aluminum layer 114 located at the bottom, thereby achieving a diffusion barrier between germanium and the bottom aluminum. Therefore, only the second aluminum layer 114 located at the top layer participates in the bonding. Since the second aluminum layer 114 is thinner, the first aluminum layer 112 and the second aluminum layer 114 are bonded together during the bonding process. The titanium layer in between acts as a diffusion barrier layer 113 to prevent the molten metal germanium from diffusing into the first aluminum layer 112 at the bottom, thereby preventing the finally formed aluminum-germanium intermelting bonding layer 115 from being too thick. At the same time, due to the existence of the titanium layer, the stratification of aluminum-germanium in the bonding structure formed by the final germanium layer 105 and the top metal stack is more obvious, which can effectively reduce the height difference of the aluminum-germanium intermelting bonding layer 115 in different areas on the wafer, improve the thickness consistency of the bonding layer, and then effectively control the distance between the end of the finger electrode and the top metal on the base wafer 108, thereby avoiding its capacitance and frequency failure.

[0108] Furthermore, since the second aluminum layer 114 involved in eutectic bonding is thinner, less overflow of molten aluminum germanium metal occurs during the bonding process, thereby avoiding short circuit problems caused by excessive overflow of molten metal, thus preventing device failure and improving yield.

[0109] Example 4

[0110] like Fig.18 As shown, this embodiment provides a MEMS device, which can be prepared by the method of embodiment 3. The MEMS device includes:

[0111] A cap wafer 101, wherein the bottom surface of the cap wafer 101 has a plurality of openings;

[0112] The device wafer 103 is located below the cap wafer 101, the top surface of the device wafer 103 is bonded to the bottom surface of the cap wafer 101, and the device wafer 103 closes the opening to form a cavity;

[0113] The bottom surface of the device wafer 103 has a boss structure 104, and the boss structure 104 is located at the edge area of ​​the cavity; the device wafer 103 has a finger electrode structure 107, and the finger electrode structure 107 is located below the cavity;

[0114] A base wafer 108 is located below the device wafer 103 , and the top surface of the base wafer 108 has an insulating layer, and the insulating layer has a wiring layer 110 ;

[0115] The top surface of the base wafer 108 and the boss structure 104 on the bottom surface of the device wafer 103 are bonded together via a metal bonding structure;

[0116] The metal bonding structure includes a patterned first aluminum layer 112 located on the surface of the insulating layer, a diffusion barrier layer 113 located on the first aluminum layer 112, and an aluminum-germanium mutual melting bonding layer 115 located between the diffusion barrier layer 113 and the boss structure 104, wherein the first aluminum layer 112 is electrically connected to the wiring layer 110;

[0117] refer to Figure 16-Figure 18 In this embodiment, the Al-Ge intermelting bonding layer 115 is formed by the intermelting of the Ge layer 105 located on the surface of the boss structure 104 and the second Al layer 114 located on the diffusion barrier layer 113 .

[0118] The material of the diffusion barrier layer 113 is titanium. Preferably, the thickness of the second aluminum layer 114 before bonding is The thickness of the first aluminum layer 112, the diffusion barrier layer 113 and the second aluminum layer 114 is The thickness of the germanium layer 105 is not less than the thickness of the second aluminum layer 114. The thickness ratio of the germanium layer 105 to the second aluminum layer 114 can be selected according to the process requirements. The thickness range of the titanium layer is The thickness of the first aluminum layer 112 is in the range of In the metal bonding structure (ie after bonding), the thickness of the second aluminum layer 114 is

[0119] The MEMS device of this embodiment is a gyroscope. In the MEMS device of this embodiment, the top metal stack on the base wafer 108 adopts an aluminum-titanium-aluminum sandwich structure. Since metal titanium cannot react with metal aluminum or germanium eutectic, the titanium layer can effectively block the germanium layer 105 from diffusing to the second aluminum layer 114 located at the bottom during the eutectic bonding process, thereby achieving a diffusion barrier between germanium and the bottom aluminum. During the bonding process, only the second aluminum layer 114 located at the top of the top metal stack is used to bond with the germanium layer 105 on the first substrate 100. Since the thickness of the second aluminum layer 114 is thinner, only Therefore, the thickness of the aluminum-germanium mutual melting bonding layer 115 formed at last is thinner, which can be more conducive to controlling the thickness consistency of the aluminum-germanium mutual melting bonding layer 115 in different areas on the wafer, and then effectively controlling the distance between the end of the finger and the top metal layer, ensuring that the capacitance and frequency will not fail. In addition, it is less likely to produce excessive metal overflow during the bonding process, which can avoid problems such as circuit short circuit caused by overflow, and the device function is not easy to fail. Therefore, the MEMS device of this embodiment can have better functional stability.

[0120] It should be noted that the various embodiments in this specification are described in a related manner, and the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the structural embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.

[0121] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A bonding method, characterized in that: include: providing a first substrate; forming a patterned germanium layer on the front side of the first substrate; providing a second substrate; forming a patterned top metal stack on the front side of the second substrate, the top metal stack comprising a first aluminum layer on the second substrate, a diffusion barrier layer on the first aluminum layer, and a second aluminum layer on the diffusion barrier layer; aligning the germanium layer on the front side of the first substrate with the top metal layer on the front side of the second substrate; The second aluminum layer and the germanium layer are bonded together to form an aluminum-germanium mutual melting bonding layer.

2. The bonding method according to claim 1, characterized in that: The material of the expansion barrier layer is titanium.

3. The bonding method according to claim 1, characterized in that: The thickness of the top metal stack is The thickness of the second aluminum layer before bonding is The thickness of the second aluminum layer after bonding is 4. The bonding method according to claim 1, characterized in that: bonding the second aluminum layer and the germanium layer together through a eutectic bonding process; The process conditions adopted in the eutectic bonding process include: Bonding temperature: 400-500℃; Bonding time: 5-15min; Bonding pressure: 5000-7000mpa.

5. A bonding structure, characterized in that: include: a first substrate; A second substrate is located below the first substrate, and a top surface of the second substrate is bonded to a bottom surface of the first substrate via a metal bonding structure; The metal bonding structure includes a patterned first aluminum layer located on the top surface of the second substrate, a diffusion barrier layer located on the first aluminum layer, and an aluminum-germanium mutual melting bonding layer located between the diffusion barrier layer and the first substrate; The aluminum-germanium mutual melting bonding layer is formed by mutual melting of a patterned germanium layer located on the bottom surface of the first substrate and a second aluminum layer located on the diffusion barrier layer.

6. The bonding structure according to claim 5, characterized in that: The material of the diffusion barrier layer is titanium.

7. The bonding structure according to claim 5, characterized in that: The sum of the thicknesses of the first aluminum layer, the diffusion barrier layer, and the second aluminum layer is The thickness of the second aluminum layer before bonding is The thickness of the second aluminum layer in the metal bonding structure is 8. A method for manufacturing a MEMS device, characterized in that: include: Providing a cap wafer, wherein a plurality of openings are formed on the front side of the cap wafer; Providing a device wafer, bonding the front side of the device wafer to the front side of the cap wafer, wherein the device wafer closes the opening to form a cavity; Etching the back side of the device wafer to form a boss structure on the back side of the device wafer, wherein the boss structure is located at an edge region of the cavity; forming a germanium layer on the top surface of the boss structure; forming an interdigitated electrode structure in the device wafer, wherein the interdigitated electrode structure is located above the cavity; Providing a base wafer, wherein an insulating layer is formed on the front side of the base wafer, and a wiring layer is formed in the insulating layer; Forming a patterned top metal stack on the insulating layer, the top metal stack is electrically connected to the wiring layer, the top metal stack comprising a first aluminum layer located on the surface of the insulating layer, a diffusion barrier layer located on the first aluminum layer, and a second aluminum layer located on the diffusion barrier layer; aligning the boss structure on the back side of the device wafer with the top metal stack on the substrate wafer; The second aluminum layer and the germanium layer are bonded together to form an aluminum-germanium mutual melting bonding layer.

9. The method for manufacturing a MEMS device according to claim 8, characterized in that: The material of the diffusion barrier layer is titanium.

10. The method for manufacturing a MEMS device according to claim 8, characterized in that: The thickness of the top metal stack is The thickness of the second aluminum layer before bonding is The thickness of the second aluminum layer after bonding is 11. The method for manufacturing a MEMS device according to claim 8, characterized in that: The material of the wiring layer is aluminum.

12. The method for manufacturing a MEMS device according to claim 8, characterized in that: bonding the second aluminum layer and the germanium layer together through a eutectic bonding process; The process conditions adopted in the eutectic bonding process include: Bonding temperature: 400-500℃; Bonding time: 5-15min; Bonding pressure: 5000-7000mpa.

13. The method for manufacturing a MEMS device according to claim 8, characterized in that: Before etching the back side of the device wafer to form a boss structure, the method further includes: The back side of the device wafer is thinned.

14. A MEMS device, characterized in that: include: A cap wafer, wherein the bottom surface of the cap wafer has a plurality of openings; A device wafer is located below the cap wafer, the top surface of the device wafer is bonded to the bottom surface of the cap wafer, and the device wafer closes the opening to form a cavity; The bottom surface of the device wafer has a boss structure, and the boss structure is located in the edge area of ​​the cavity; the device wafer has an interdigitated electrode structure, and the interdigitated electrode structure is located below the cavity; A base wafer is located below the device wafer, the top surface of the base wafer has an insulating layer, and the insulating layer has a wiring layer; The top surface of the base wafer and the boss structure on the bottom surface of the device wafer are bonded together via a metal bonding structure; The metal bonding structure comprises a patterned first aluminum layer located on the surface of the insulating layer, a diffusion barrier layer located on the first aluminum layer, and an aluminum-germanium mutual melting bonding layer located between the diffusion barrier layer and the boss structure, wherein the first aluminum layer is electrically connected to the wiring layer; The aluminum-germanium mutual melting bonding layer is formed by mutual melting of a germanium layer located on the surface of the boss structure and a second aluminum layer located on the diffusion barrier layer.

15. The MEMS device according to claim 14, characterized in that: The material of the diffusion barrier layer is titanium.

16. The MEMS device according to claim 14, characterized in that: The sum of the thicknesses of the first aluminum layer, the diffusion barrier layer, and the second aluminum layer is The thickness of the second aluminum layer before bonding is The thickness of the second aluminum layer in the metal bonding structure is