Preparation method and application of iron phosphate positive electrode material for magnesium battery
By adding acid liquid and reducing gas to the lithium extraction slag for leaching, and combining the precipitation reactions of iron, aluminum and phosphorus sources, the problems of large acid and alkali use and low leaching efficiency were solved, and high porosity FePO4 was prepared , used in magnesium ion batteries, improving the magnesium storage performance of magnesium ion batteries.
Patent Information
- Application Number
- CN202411159822.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The prior art uses large acid and alkali, low leaching efficiency, high product impurity content, low recovery rate of phosphorus and iron resources, and poor Mg2+ in FePO4 positive electrode materials.
A method for preparing iron phosphate positive electrode material for magnesium batteries, including adding acid solution to lithium extraction slag and introducing reducing gas for strengthening and leaching, followed by adding iron, aluminum and phosphorus sources for precipitation reaction, and controlling pH value And the acid solution etching treatment was performed to obtain FePO4 with high pores and defects, which was used to prepare the aqueous magnesium ion battery electrode material.
It significantly reduces the leaching cost, improves the leaching efficiency, realizes the battery-level purity and excellent electronic conductivity of FePO4, shortens the Mg2+ diffusion path, and improves the magnesium storage performance of magnesium ion batteries.
Smart Images

Figure BDA0005006117100000042 
Figure BDA0005006117100000071 
Figure BDA0005006117100000072
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of recycling and comprehensive utilization of solid waste resources, and specifically to a preparation method and application of an iron phosphate positive electrode material for a magnesium battery. Background Art
[0002] Lithium iron phosphate batteries stand out from many lithium-ion batteries with their lower cost, better stability and longer cycle life. With the vigorous development of the new energy vehicle industry, the demand for lithium iron phosphate batteries has exploded, and the number of waste lithium iron phosphate batteries will also increase year by year. How to efficiently recycle waste lithium iron phosphate batteries has become a research focus and hotspot in recent years.
[0003] As lithium is the most valuable element in spent lithium iron phosphate batteries, most studies focus on recovering lithium resources from spent lithium iron phosphate batteries. Currently, oxidative leaching technology has been proven to be useful for the selective extraction of lithium. 2 O 2 、Na 2 S 2 O 8 , O 3 LiFePO 4 Oxidized to FePO 4 , and Li + Leaching into the solution. Compared with the complete leaching technology, the selective lithium extraction technology can minimize the loss of lithium, thereby improving the recovery rate of lithium. However, this technology will produce lithium extraction slag (LES) with high phosphorus and iron content. If it is not properly stacked, it may cause soil acidification, water eutrophication and other hazards. Therefore, the effective recovery of LES is very important. In recent years, some companies have mainly used wet processes to treat LES. This process generally uses high-concentration sulfuric acid, hydrochloric acid or phosphoric acid and other inorganic acids to remove FePO in LES. 4 After purification and impurity removal, the pH is adjusted by adding sodium hydroxide or ammonia to make FePO 4 Although this method can achieve FePO 4 However, the process requires large amounts of acid and alkali, has low leaching efficiency, and also has problems such as high impurity content in the product and low recovery rate of ferrophosphorus resources due to the lack of an effective impurity removal step.
[0004] FePO recovered from lithium extraction slag 4 It is mainly used to synthesize lithium iron phosphate and continues to serve as the positive electrode material of lithium-ion batteries. However, the current lithium resources are becoming increasingly depleted and unevenly distributed, which leads to an increasing cost for the synthesis of lithium iron phosphate. Compared with lithium-ion batteries, magnesium-ion batteries not only have higher safety and lower cost, but also have a larger volume specific capacity. Existing research has shown that FePO 4It has the potential to be used as an electrode material for magnesium ion batteries, but there is Mg 2+ Problems such as poor insertion / extraction performance and poor electronic conductivity ultimately affect the performance of magnesium-ion batteries. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of this application is to provide a method for preparing an iron phosphate positive electrode material for a magnesium battery and its application, so as to solve the problem of recovering FePO4 from LES in the prior art. 4 The amount of acid and alkali used is large, the leaching efficiency is low, the product impurity content is high, the recovery rate of phosphorus and iron resources is low, and Mg 2+ In FePO 4 The problem of poor insertion / extraction performance in the positive electrode material. The FePO synthesized in this application 4 ·H 2 O can reach battery-grade purity and has a large number of pores and defects, which is beneficial to improve the electronic conductivity of the material and shorten the Mg 2+ The diffusion path into the material increases the Mg 2+ Diffusion rate.
[0006] In order to solve the above technical problems, this application adopts the following technical solutions:
[0007] A method for preparing an iron phosphate positive electrode material for a magnesium battery comprises the following steps:
[0008] Step 1: After adding acid solution to the lithium extraction slag, a reducing gas is introduced to perform enhanced leaching to obtain carbon slag and a leaching solution; wherein the molar ratio of hydrogen ions in the acid solution to iron in the lithium extraction slag is (0.2-5):1; the leaching temperature is 25-90° C., and the leaching time is 10-240 min;
[0009] Step 2: Add iron source, aluminum source and phosphorus source to the leaching solution, adjust the pH value to make the pH value <5.5, and add oxidant for precipitation reaction. After the reaction is completed, filter to obtain FePO 4 ·2H 2 O@Al(OH) 3 Precursor; wherein the molar ratio of phosphorus in the phosphorus source to iron in the iron source is 0.9 to 1.8, and the molar ratio of aluminum in the aluminum source to iron in the iron source is 0.02 to 3; the precipitation reaction temperature is 25 to 90° C., and the precipitation reaction time is 30 to 360 min;
[0010] Step 3: The precursor obtained in step 2 is sequentially subjected to acid solution etching, water washing, drying and dehydration treatment to obtain the FePO 4 .
[0011] Preferably, the lithium extraction slag is the solid residue remaining after lithium element is extracted from the lithium-containing raw material.
[0012] Preferably, the lithium extraction slag is the lithium extraction slag obtained by subjecting waste lithium iron phosphate battery black powder to lithium extraction treatment.
[0013] Preferably, in step 1, the acid solution is at least one of sulfuric acid, nitric acid or hydrochloric acid, and the hydrogen ion concentration in the acid solution is 0.2 to 3 mol / L; the reducing gas is SO 2 , NO or HCl, the flow rate of the reducing gas is 0.02-2 L / min, and the introduction time of the reducing gas is consistent with the leaching time.
[0014] Preferably, in step 2, the iron source is ferric sulfate, the aluminum source is aluminum sulfate, and the phosphorus source is at least one of phosphoric acid, sodium phosphate or potassium phosphate; the oxidant is at least one of oxygen, air, chlorine or hydrogen peroxide; the amount of the oxidant added (the amount of the oxidant) is 0.8 to 2 times the amount of the iron in the leachate; and the pH value is controlled at 0.5 to 5.5.
[0015] Preferably, in step 3, the acid solution is at least one of sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, formic acid or acetic acid, and the hydrogen ion concentration in the acid solution is 0.05 to 1.2 mol / L, and the acid solution can be repeatedly used; wherein the etching temperature of the acid solution is 30 to 180° C., and the etching time is 20 to 360 min.
[0016] The present application provides an application of an iron phosphate positive electrode material. The FePO prepared by the above method 4 Used to prepare electrode materials for aqueous magnesium ion batteries.
[0017] Preferably, the method for preparing the electrode material comprises the following steps:
[0018] Conductive material, polyvinylidene fluoride and FePO 4 After mixing in a mass ratio of (1-3):(1-2):(6-8), adding into N-methylpyrrolidone to prepare electrode slurry, coating the electrode slurry on a current collector, and drying at 80-100° C. to obtain an aqueous magnesium ion battery electrode sheet.
[0019] Preferably, the conductive material is at least one of acetylene black, Super P, carbon nanotubes, and graphene, and the fluid is at least one of carbon cloth or carbon paper.
[0020] Compared with the prior art, this application has the following beneficial effects:
[0021] 1. The present application enhances the leaching effect by introducing reducing gas during the leaching process. The introduction of reducing gas not only provides a reducing atmosphere, but also improves the material exchange efficiency of the reaction. Compared with the traditional high-concentration acid solution leaching method and the reduction leaching method with the addition of iron powder or sulfide, the present application significantly reduces the leaching temperature, acid dosage, acid concentration and time, thereby saving leaching costs and improving leaching efficiency.
[0022] 2. This application is based on FePO 4 The aluminum impurities were retained during the precipitation process and induced to react with FePO 4 Co-precipitation, followed by acid solution etching to remove aluminum impurities and create pores in the material, the synthesized FePO 4 Not only can it achieve battery-grade purity, but it also has a large number of pores and defects, which is beneficial to improve the electronic conductivity of the material and shorten the Mg 2+ The diffusion path into the material increases the Mg 2+ The diffusion rate is very fast. When it is used as an electrode material for aqueous magnesium ion batteries, it has excellent magnesium storage performance and exhibits a capacity of 180 mAh / g in 1M magnesium chloride electrolyte aqueous solution.
[0023] 3. This application uses solid waste from the battery recycling field as raw materials to prepare electrode materials suitable for aqueous magnesium ion batteries, thereby realizing the resource recycling and comprehensive utilization of solid waste. DETAILED DESCRIPTION
[0024] This application will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on this application belong to the scope of protection of this application.
[0025] Unless otherwise indicated in specific cases in this application, the numerical ranges listed herein include the upper and lower limits, as well as all integers and fractions within the range, and are not limited to the specific values listed when defining the range.
[0026] 1. A method for preparing an iron phosphate positive electrode material for a magnesium battery
[0027] Step 1: After adding acid solution to the lithium extraction slag, a reducing gas is introduced to perform enhanced leaching to obtain carbon slag and leachate.
[0028] Step 2: Add iron source, aluminum source and phosphorus source to the leaching solution, adjust the pH value to make the pH value <5.5, and add oxidant for precipitation reaction. After the reaction is completed, filter to obtain FePO 4 ·2H 2 O@Al(OH) 3 Precursor.
[0029] Step 3: The precursor obtained in step 2 is sequentially subjected to acid solution etching, water washing, drying and dehydration treatment to obtain a high-porosity amorphous FePO 4 .
[0030] The present invention introduces reducing gas into the leaching process and finds that the introduction of reducing gas can not only improve the material exchange efficiency in the reaction, but also significantly reduce the leaching temperature, acid dosage, acid concentration and time compared with the traditional high-concentration acid solution leaching method and the reduction leaching method with the addition of iron powder or sulfide, thereby greatly reducing the leaching cost and improving the leaching efficiency. At the same time, the present invention also unexpectedly found that in FePO 4 During the precipitation process, the aluminum impurities are retained and induced to react with FePO 4 The co-precipitation and then the removal of aluminum impurities by acid solution etching can achieve pore formation of the material. Moreover, the FePO obtained in this way 4 The material can not only achieve battery-grade purity, but also has a large number of pores and defects in its structure, which is very beneficial to improve the electronic conductivity of the material, especially in the application of aqueous magnesium ion batteries. This structure can significantly shorten the Mg 2+ Diffusion path into the material, thereby increasing Mg 2+ Diffusion rate, has very good application prospects.
[0031] In some embodiments of the present application, the lithium extraction slag described in the present application may be a solid residue remaining after lithium is extracted from a lithium-containing raw material. Specifically, the lithium extraction slag from waste lithium iron phosphate battery is the lithium extraction slag remaining after selective lithium extraction from waste lithium iron phosphate battery black powder by oxidative acid leaching, and the lithium extraction slag mainly includes iron phosphate, graphite, conductive carbon, binder, and copper and aluminum metal impurities.
[0032] In some embodiments of the present application, in step 1, the acid solution is an aqueous solution of an acidic substance, for example, sulfuric acid is a solution containing H 2 SO 4 of aqueous solution. In step 1, the acid solution is at least one of sulfuric acid, nitric acid or hydrochloric acid, and the hydrogen ion concentration in the acid solution is 0.2 to 3 mol / L. The hydrogen ion concentration in the acid solution is controlled within this range in order to reduce the leaching cost while ensuring the leaching effect. Therefore, the hydrogen ion concentration in the acid solution can be 0.2 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0033] In some embodiments of the present application, in step 1, the molar ratio of hydrogen ions in the acid solution to iron in the lithium extraction slag is (0.2-5):1. The molar ratio of hydrogen ions in the acid solution to iron in the lithium extraction slag is controlled within this range in order to reduce the leaching cost while ensuring the leaching effect. Therefore, the molar ratio of hydrogen ions in the acid solution to iron in the lithium extraction slag is preferably (0.8-5):1, which can be 0.2, 0.5, 0.8, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0034] In some embodiments of the present application, in step 1, the reducing gas is SO 2 , NO or HCl, the flow rate of the reducing gas is 0.02-2 L / min, and the introduction time of the reducing gas is consistent with the leaching time. The type of reducing gas corresponds to the type of acid solution, that is, when the acid solution is sulfuric acid, the reducing gas is SO 2 ; Similarly, when the acid is nitric acid, the reducing gas is NO; when the acid is hydrochloric acid, the reducing gas is HCl. The use of different types of acid and reducing gas has a significant effect on the leaching rate of iron and phosphorus. The sulfuric acid / sulfur dioxide system has a better leaching effect, followed by the hydrochloric acid / hydrogen chloride system, and finally the nitric acid / nitric oxide system. Although different acid / reducing gas systems have a significant effect on the leaching rate of iron and phosphorus, high-porosity FePO can still be successfully prepared. 4 , but the yield of the product will be affected. When the reducing gas introduced is sulfur dioxide, the reactions occurring in the leaching process include:
[0035]
[0036] Cu+2H + →Cu 2+ +H 2
[0037]
[0038] Therefore, the reducing gas is further preferably sulfur dioxide. It should be understood that, in embodiments, any of the above ranges may be combined with any other ranges.
[0039] In some embodiments of the present application, in step 1, the leaching temperature is 25 to 90°C, and the leaching time is 10 to 240 min. Too low a leaching temperature will have an adverse effect on the leaching effect, while too high a leaching temperature will increase the leaching cost, which is not conducive to actual industrial production. The leaching temperature can be 25°C, 40°C, 50°C, 70°C, 80°C, 90°C, etc., and all ranges and sub-ranges between the above values; too short a leaching time will have an adverse effect on the leaching effect; and too long a leaching time will increase the leaching cost, which is not conducive to actual industrial production. Therefore, the leaching time can be 10 min, 30 min, 60 min, 120 min, 180 min, 240 min, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0040] In some embodiments of the present application, in step 2, an aluminum source is added to the leachate in order to synthesize iron phosphate containing a certain amount of aluminum impurities, which are embedded in the structure of the iron phosphate to provide etching sites for the acid etching step in step 3, thereby preparing amorphous iron phosphate containing holes and defects. Since the aluminum, iron and phosphorus contents in different batches of leachate are different, in order to ensure that the composition of the precipitated iron phosphate containing aluminum impurities is uniform, an aluminum source, an iron source or a phosphorus source needs to be appropriately added to the leachate. The iron source is ferrous sulfate, the aluminum source is aluminum sulfate, and the phosphorus source is at least one of phosphoric acid, sodium phosphate or potassium phosphate.
[0041] In some embodiments of the present application, in step 2, the molar ratio of phosphorus in the phosphorus source to iron in the iron source is 0.9 to 1.8. A phosphorus-iron molar ratio that is too low will result in the precipitation of byproduct iron hydroxide, and a high phosphorus-iron molar ratio will result in the precipitation of byproduct iron pyrophosphate. Therefore, the phosphorus-iron molar ratio can be 0.9, 1.0, 1.3, 1.5, 1.8, etc., and all ranges and sub-ranges between the above values; the molar ratio of aluminum in the aluminum source to iron in the iron source is 0.02 to 3. A too low aluminum-iron molar ratio indicates that the aluminum element is insufficient, which will affect FePO 4 The formation of pores and defects in the structure has an adverse effect, resulting in a decrease in porosity; and the aluminum-iron molar ratio is too high, which will make FePO 4 The number of pores and defects in the structure is too large, which makes FePO 4 The structure is unstable and it is difficult to meet the use requirements of ion batteries. Therefore, it is further preferably 0.05 to 3, and can be 0.02, 0.05, 0.1, 0.5, 0.8, 1.0, 1.5, 2.0, 2.5, 3.0, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0042] In some embodiments of the present application, in step 2, the oxidant is at least one of oxygen, air, chlorine or hydrogen peroxide; the amount of the oxidant added (the amount of the oxidant substance) is 0.4 to 2 times the amount of the iron substance in the leachate. Subsequently, the pH value is adjusted by adding an alkali (such as sodium hydroxide, ammonia water, sodium carbonate, etc.). If the pH value is too low, the precipitation rate of the aluminum element is lower, resulting in fewer acid etching points in step 3, so the porosity and defects of the material are less, and the lower the pH value, the lower the precipitation rate of iron, resulting in the recovery of FePO 4 As the pH value increases, impurities such as Cu, Co, and Ni in the leaching solution will precipitate, which will affect the FePO 4 The purity of the material will decrease, so the pH value is not easy to be higher than 5.5. The iron phosphate prepared at or above 5.5 will be difficult to meet the requirements of battery-grade iron phosphate. The pH value is adjusted to 0.5-5.5, more preferably 1.5-4.5, which can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0043] In some embodiments of the present application, in step 2, the precipitation reaction temperature is 25 to 90°C, and the precipitation reaction temperature can be 25°C, 40°C, 50°C, 70°C, 80°C, 90°C, etc., and all ranges and sub-ranges between the above values. The precipitation reaction time is 30 to 360 min, and the precipitation reaction time can be 30 min, 60 min, 120 min, 180 min, 240 min, 300 min, 360 min, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0044] In some embodiments of the present application, in step 3, the acid solution etching can remove FePO 4 ·2H 2 O@Al(OH) 3 Al(OH) in the precursor 3 Impurities, the material after aluminum removal can reach battery-grade purity, and also contains a large number of holes and defects, which is beneficial to improve the electronic conductivity of the material and shorten the Mg 2+ The diffusion path into the material increases the Mg 2+Diffusion rate. The acid solution is at least one of sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, formic acid or acetic acid, and the hydrogen ion concentration in the acid solution is 0.05-1.2 mol / L, and the acid solution can be used repeatedly. Too low a hydrogen ion concentration in the acid solution will result in insufficient etching effect, too few holes and defects formed; while too high a hydrogen ion concentration will result in excessive etching time, thereby affecting the stability of the product structure. Therefore, the hydrogen ion concentration in the acid solution can be 0.2 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0045] In some embodiments of the present application, in step 3, the acid solution etching temperature is 30 to 180°C, and the acid solution etching temperature can be 30°C, 50°C, 100°C, 140°C, 170°C, 180°C, etc., and all ranges and sub-ranges between the above values. The time of acid solution etching is 20 to 360min, and the time of acid solution etching can be 20min, 60min, 120min, 180min, 240min, 300min, 360min, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0046] 2. Application of an iron phosphate positive electrode material
[0047] The FePO prepared by the method described in this application 4 It can be used to prepare aqueous magnesium ion battery electrode materials. The preparation method of the electrode material comprises the following steps:
[0048] Conductive material, polyvinylidene fluoride and FePO 4 After mixing in a mass ratio of (1-3):(1-2):(6-8), adding into N-methylpyrrolidone to prepare electrode slurry, coating the electrode slurry on a current collector, and drying at 80-100° C. to obtain an electrode sheet for an aqueous magnesium ion battery. The conductive material is at least one of acetylene black, Super P, carbon nanotubes, and graphene, and the fluid is at least one of carbon cloth or carbon paper.
[0049] 3. Examples and Comparative Examples
[0050] The LES used in the following embodiments and comparative examples of the present application is the residue after selective lithium extraction from waste lithium iron phosphate batteries by oxidative acid leaching. The elemental composition of the black powder of waste lithium iron phosphate batteries is shown in Table 1, and the elemental composition of LES is shown in Table 2.
[0051] Table 1
[0052] element C P Fe Cu Al Li Content (wt.%) 30.5 11.3 18.0 3.4 2.3 3.0
[0053] Table 2
[0054] element C P Fe Cu Al Li Content (wt.%) 31.1 11.7 19.9 3.6 2.2 0.2
[0055] Embodiment 1:
[0056] Step 1: add 100 g of LES into water, add 1.2 mol / L sulfuric acid, and control the molar ratio of hydrogen ions in the added acid to iron in LES to be 1:1, introduce sulfur dioxide at a rate of 0.45 L / min and leaching at 60°C for 30 min, and filter to obtain a leachate after the leaching is completed;
[0057] Step 2: Add ferric sulfate, aluminum sulfate and sodium phosphate to the impurity removal filtrate, control the phosphorus-iron molar ratio in the impurity removal filtrate to be 1.2, the aluminum-iron molar ratio to be 0.1, introduce oxygen at a rate of 0.45 L / min, adjust the pH to 1.5, control the reaction temperature to 40°C, the reaction time to 60 min, and filter after the reaction to obtain FePO 4 ·2H 2 O@Al(OH) 3 Precursor;
[0058] Step 3: Etch FePO4 with 1 mol / L phosphoric acid solution at 60 °C 4 ·2H 2 O@Al(OH) 3 The precursor was filtered after 30 minutes, and then washed, dried and calcined to remove water to obtain FePO 4 Material.
[0059] The iron and phosphorus contents in the leaching solution in step 1 were tested by ICP-OES and the leaching rate was calculated; the precipitated FePO4 in step 2 was tested by ICP-OES. 4 ·2H 2 O@Al(OH) 3 The contents of iron, copper and aluminum in the solution before and after the precursor were measured and the precipitation rates of iron, copper and aluminum were calculated; the FePO4 after calcination and dehydration in step 3 was tested by BET and powder metallurgy density meter. 4 The porosity of the material is determined according to the detection method of HG / T 4701-2014. 4 ·2H 2 O material, the above ICP-OES test and BET test results are shown in Table 3, FePO before calcination and dehydration 4 ·2H 2 The comparison between O material and the technical standard of battery-grade iron phosphate (HG / T 4701-2014) is shown in Table 4.
[0060] Table 3
[0061]
[0062] Table 4
[0063]
[0064]
[0065] Take 0.8 g of FePO obtained in step 4 of Example 1 4 The material was dispersed in NMP with 0.1 g acetylene black and 0.1 g PVDF to make a slurry and evenly coated on the carbon cloth. The slurry was placed in a vacuum oven at 80 °C to obtain an electrode sheet. The electrochemical performance was tested by three-electrode electrochemistry. The working electrode was FePO 4 The counter electrode and reference electrode were graphite and silver / silver chloride respectively, the electrode liquid was 1M magnesium chloride aqueous solution, and the constant current charge-discharge test technology was used to determine the recovered FePO 4 It has a charge and discharge capacity of >180mAh / g.
[0066] Embodiment 2~6:
[0067] The changes of some parameters of Examples 2 to 6 are shown in Table 5, and the remaining parameters are the same as those of Example 1. The test results are shown in Table 6.
[0068] Table 5
[0069]
[0070] Table 6
[0071]
[0072] The above embodiments are all implemented under the conditions described in the present invention. The data such as leaching rate and precipitation rate under different conditions are slightly different. The synthesized iron phosphate meets the technical standard of battery-grade iron phosphate (HG / T 4701-2014). FePO 4 The magnesium storage performance is mainly related to the conditions of step 2 and step 3, and the charge and discharge capacity is related to FePO 4 is proportional to the porosity.
[0073] Embodiment 7:
[0074] 100 g of LES was added into water, and 1 mol / L hydrochloric acid was added, and the molar ratio of hydrogen ions in the added acid to iron in LES was controlled to be 1:1. Hydrogen chloride was introduced at a rate of 0.45 L / min and leached at 60°C for 30 min. After the leaching was completed, the leachate was filtered to obtain the leachate. The iron and phosphorus contents in the leachate were tested by ICP-OES and the leaching rate was calculated.
[0075] Embodiment 8:
[0076] 100 g of LES was added into water, 1 mol / L nitric acid was added, and the molar ratio of hydrogen ions in the acid to iron in LES was controlled to be 1:1. Nitric oxide was introduced at a rate of 0.45 L / min and leached at 60°C for 30 min. After leaching, the leachate was filtered to obtain the leachate. The iron and phosphorus contents in the leachate were tested by ICP-OES and the leaching rate was calculated.
[0077] Comparative Example 1:
[0078] 100 g of LES was added into water, 1 mol / L sulfuric acid was added, and the molar ratio of hydrogen ions in the added acid to iron in LES was controlled to be 1:1. Leaching was carried out at 60°C for 30 min. After leaching, the leachate was filtered to obtain the leachate. The iron and phosphorus contents in the leachate were tested by ICP-OES and the leaching rate was calculated.
[0079] The test results of Example 7, Example 8 and Comparative Example 1 are shown in Table 7.
[0080] Table 7
[0081]
[0082] By comparing Example 1, Example 7, Example 8 and Comparative Example 1, it can be found that the sulfuric acid / sulfur dioxide leaching system has a higher leaching rate than the hydrochloric acid / hydrogen chloride and nitric acid / nitric oxide leaching systems, and the introduction of sulfur dioxide can significantly increase the leaching rate of iron and phosphorus. The leachate obtained in Examples 7 and 8 is subsequently treated in the same steps 2 and 3 as in Example 1, and high-porosity iron phosphate can still be obtained.
[0083] Embodiments 9 to 12:
[0084] The changes of some parameters of Examples 9 to 12 and Comparative Example 2 are shown in Table 8, and the remaining parameters are the same as those of Example 1. The test results are shown in Table 9.
[0085] Table 8
[0086]
[0087]
[0088] Table 9
[0089]
[0090] By comparing Example 1, Examples 9 to 12 and Comparative Example 2, it can be found that:
[0091] (1) Compared with Example 2, the examples can meet the standards of battery-grade iron phosphate and have relatively high charge and discharge capacities.
[0092] (2) In combination with Examples 1 to 3 and Examples 8 and 9, the addition amount of sulfuric acid and the low sulfuric acid concentration in step 1 will affect the leaching rate of phosphorus and iron, but will not have a significant effect on the porosity of iron phosphate. The iron phosphate prepared in Examples 9 and 10 still has a relatively high porosity. This also shows that the leaching effect does not affect the formation of pores and defects inside the iron phosphate.
[0093] (3) In combination with Examples 4 to 5, Example 11 and Comparative Example 2, the low aluminum content in step 2 and the high precipitation pH both affect the synthesized FePO 4 The porosity affects the charge and discharge capacity of the material. Especially in comparative example 2, even though it has a higher charge and discharge capacity, it does not meet the standard of battery iron phosphate.
[0094] (4) In combination with Examples 6 and 12, the low hydrogen ion concentration in the acid solution used for etching in step 3 will affect the FePO 4 ·2H 2 O@Al(OH) 3 The removal rate of aluminum impurities in the precursor affects FePO 4 porosity.
[0095] The changes of some parameters of Comparative Examples 3 to 10 are shown in Table 10, and the remaining parameters are the same as those of Example 1. The test results are shown in Table 11.
[0096] Table 10
[0097]
[0098]
[0099] Table 11
[0100]
[0101] Comparing Examples 1 to 12 with Comparative Examples 3 to 10, it can be seen that:
[0102] (1) It can be seen from Comparative Examples 3 and 4 that the molar ratio of hydrogen ions in the acid to iron in the LES and the concentration of hydrogen ions in the acid have a significant effect on the leaching effect of iron and phosphorus in step 1.
[0103] (2) It can be seen from Comparative Examples 5 and 6 that the aluminum-iron molar ratio is not within the scope of the present application, which will cause the iron phosphate to show significant differences in porosity. When applied to magnesium ion batteries, the difference in electrochemical performance will be more obvious.
[0104] (3) It can be seen from Comparative Examples 7 and 8 that a phosphorus-iron molar ratio that is too low or too high will have a very adverse effect on the charge and discharge capacity. This is because a phosphorus-iron molar ratio that is too low will cause the by-product iron hydroxide to precipitate, which in turn causes the by-product to enter the iron phosphate material; while a phosphorus-iron molar ratio that is too high will also cause the by-product iron pyrophosphate to precipitate, resulting in insufficient purity of the iron phosphate. The iron phosphate prepared in these two cases cannot meet the battery-grade iron phosphate standard.
[0105] (4) It can be seen from Comparative Examples 9 and 10 that too low or too high a hydrogen ion concentration in the acid solution will have an adverse effect on the prepared iron phosphate, resulting in it being unable to meet the standards for battery-grade iron phosphate.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the technical solution. Ordinary technicians in this field should understand that those modifications or equivalent substitutions of the technical solution of the present application that do not depart from the purpose and scope of the technical solution of the present application should be included in the scope of the claims of the present application.
Claims
1. A method for preparing an iron phosphate positive electrode material for a magnesium battery, characterized in that: The specific steps include: Step 1: After adding acid solution to the lithium extraction slag, a reducing gas is introduced to perform enhanced leaching to obtain carbon slag and a leaching solution; wherein the molar ratio of hydrogen ions in the acid solution to iron in the lithium extraction slag is (0.2-5):1; the leaching temperature is 25-90° C., and the leaching time is 10-240 min; Step 2: adding an iron source, an aluminum source and a phosphorus source to the leaching solution, adjusting the pH value to make the pH value less than 5.5, and adding an oxidant for precipitation reaction, filtering after the reaction to obtain a FePO4·2H2O@Al(OH)3 precursor; wherein the molar ratio of phosphorus in the phosphorus source to iron in the iron source is 0.9-1.8, and the molar ratio of aluminum in the aluminum source to iron in the iron source is 0.02-3; the precipitation reaction temperature is 25-90°C, and the precipitation reaction time is 30-360min; Step 3: The precursor obtained in step 2 is sequentially etched with an acid solution, washed with water, dried and dehydrated to obtain the FePO4.
2. The preparation method according to claim 1, characterized in that: The lithium extraction slag is the solid residue remaining after lithium is extracted from the lithium-containing raw material.
3. The preparation method according to claim 2, characterized in that: The lithium extraction slag is the lithium extraction slag obtained after lithium extraction treatment of waste lithium iron phosphate battery black powder.
4. The preparation method according to claim 1, characterized in that: In step 1, the acid solution is at least one of sulfuric acid, nitric acid or hydrochloric acid, and the hydrogen ion concentration in the acid solution is 0.2-3 mol / L; the reducing gas is at least one of SO2, NO or HCl, the flow rate of the reducing gas is 0.02-2 L / min, and the introduction time of the reducing gas is consistent with the leaching time.
5. The preparation method according to claim 1, characterized in that: In step 2, the iron source is ferric sulfate, the aluminum source is aluminum sulfate, and the phosphorus source is at least one of phosphoric acid, sodium phosphate or potassium phosphate; the oxidant is at least one of oxygen, air, chlorine or hydrogen peroxide; the amount of the oxidant added is 0.4 to 2 times the amount of iron in the leachate; and the pH value is controlled at 0.5 to 5.
5.
6. The preparation method according to claim 1, characterized in that: In step 3, the acid solution is at least one of sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, formic acid or acetic acid, and the hydrogen ion concentration in the acid solution is 0.05-1.2 mol / L, and the acid solution can be repeatedly used; the etching temperature of the acid solution is 30-180° C., and the etching time is 20-360 min.
7. An application of an iron phosphate positive electrode material, characterized in that: The iron phosphate prepared by any of the preparation methods described in claims 1 to 6 is used to prepare electrode materials for aqueous magnesium ion batteries.
8. The use according to claim 7, characterized in that: The preparation method of the electrode material comprises the following steps: Conductive material, polyvinylidene fluoride and FePO4 are mixed in a mass ratio of (1-3):(1-2):(6-8), added into N-methylpyrrolidone to prepare an electrode slurry, the electrode slurry is coated on a current collector, and dried at 80-100° C. to obtain an aqueous magnesium ion battery electrode sheet.
9. The use according to claim 8, characterized in that: The conductive material is at least one of acetylene black, Super P, carbon nanotubes, and graphene, and the fluid is at least one of carbon cloth or carbon paper.
Citation Information
Patent Citations
Method for removing aluminum from waste lithium iron phosphate battery powder and preparing battery-grade iron phosphate
CN115838160A
Method for preparing iron phosphate from ferrophosphorus slag obtained after lithium extraction of waste lithium iron phosphate
CN116588909A