Tremella-like ferric sodium pyrophosphate composite material as well as preparation method and application thereof
Na4Fe3(PO4)2P2O7/rGO composite material is formed through spray drying and hydrothermal reaction, and metal nanocrystals are added, which solves the problem of low conductivity of Na4Fe3(PO4)2P2O7 positive electrode material, and achieves efficient sodium ion battery cycle stability and Improved rate performance.
Patent Information
- Application Number
- CN202411411590.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The existing Na4Fe3(PO4)2P2O7 positive electrode material has low conductivity, low capacity release rate, and poor rate performance, which cannot meet the needs of sodium ion batteries.
A mixed solution of Na4Fe3(PO4)2P2O7 precursor and GO was prepared by spray drying. The Na4Fe3(PO4)2P2O7/rGO composite material was formed by hydrothermal reaction, and zinc or cobalt salt was added at high temperature to form thyroid-like phosphate pyrophosphate Iron-sodium composite material uses ultrasonic dispersion and metal nanocrystals to enhance conductivity.
The conductivity and cyclic stability of the material are significantly improved, the rate performance is optimized, the high capacity can be released at high current density, and the high efficiency is maintained in long cycles. The Coulomb efficiency reaches 99.97%, and the cycle attenuation rate is low.
Smart Images

Figure CN118929615A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of positive electrode materials for sodium ion batteries, and in particular relates to a tremella-like sodium iron phosphate pyrophosphate composite material and a preparation method and application thereof. Background Art
[0002] The global lithium resources are limited and unevenly distributed. my country's lithium resources usually exist in a co-existing form, and it is difficult to extract and purify lithium from salt lakes. However, my country's power battery and energy storage market is growing, and limited lithium resources have become a factor restricting its development. Therefore, it is urgent to seek energy storage resources with abundant reserves that can meet market demand.
[0003] The limited lithium resources and the substantial growth in demand have triggered a sharp fluctuation in the price of lithium carbonate, which has attracted the attention of various battery companies. Since 2023, the first year of sodium-ion battery development has begun, and the industrialization of sodium-ion batteries has continued to advance. However, the cathode routes of sodium-ion batteries are diversified and are constantly being improved.
[0004] The theoretical specific capacity of Na4Fe3(PO4)2P2O7 is 129mAhg -1 The operating voltage is 3.2V, and sodium carbonate, iron salt, and phosphorus source are used as raw materials. It has the advantages of being environmentally friendly, low cost, and good cycle stability. However, Na4Fe3(PO4)2P2O7 has low conductivity, low capacity release rate, and poor rate performance, which cannot meet the needs in the application process.
[0005] The Chinese patent document with publication number CN107069012A discloses a hollow spherical Na4Fe3(PO4)2P2O7 / composite positive electrode material and its preparation method. A surfactant is introduced to form spherical Na4Fe3(PO4)2P2O7 by using an emulsion soft film plate method. The carbon source (one or more of starch, citric acid, sucrose, glucose, and phenolic resin) and the surfactant introduced in the material preparation process are converted into conductive carbon materials after calcination to finally form a hollow spherical Na4Fe3(PO4)2P2O7 / C composite material with a maximum current density of 200mAg -1 , the initial capacity is 66mAhg -1 The capacity retention rate after 500 cycles is 68%. The problems are that the ability to withstand large currents is poor, the specific capacity release rate is low, and the retention rate is poor. Summary of the invention
[0006] The invention aims to provide a tremella-like sodium iron phosphate pyrophosphate composite material and a preparation method and application thereof; the prepared tremella-like sodium iron phosphate pyrophosphate composite material has good electrical conductivity and cycle stability and is suitable for sodium ion batteries.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a method for preparing a Tremella-like sodium iron phosphate pyrophosphate composite material, comprising the following steps: (1) dissolving an inorganic salt containing sodium and phosphorus, a chain carbon source and an inorganic strong acid iron salt in deionized water and stirring the mixture for reaction, and spray drying the reaction solution to obtain a Na4Fe3(PO4)2P2O7 material precursor; (2) adding Na4Fe3(PO4)2P2O7 material precursor and GO into deionized water, and ultrasonically dispersing them to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution; and performing a hydrothermal reaction to obtain a Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution; (3) Adding an inorganic strong acid zinc salt or an inorganic strong acid cobalt salt to the Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution, stirring evenly to form a suspension, filtering, washing, and drying the suspension to obtain a composite material precursor; calcining the composite material precursor in an Ar-H2 atmosphere to obtain a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / M) after calcination.
[0008] Furthermore, in the step (1), the inorganic salt containing sodium and phosphorus is sodium hypophosphite or sodium dihydrogen phosphate; the inorganic strong acid iron salt is ferric nitrate or ferric chloride; the chain carbon source is glucose or citric acid; the molar ratio of the inorganic salt containing sodium and phosphorus, the inorganic strong acid iron salt, and the chain carbon source is 0.4 mol: 0.29-0.31 mol: 0.03-0.05 mol; the spray drying temperature is 110-150°C; and the flow rate is 200-300 mL / h -1 .
[0009] Furthermore, in the step (2), the mass ratio of the added Na4Fe3(PO4)2P2O7 material precursor to GO is 10-20:1; the hydrothermal reaction temperature is 150-180°C; and the hydrothermal reaction is for 15-24h.
[0010] Furthermore, in the step (3), the added inorganic strong acid zinc salt is zinc chloride or zinc nitrate; the inorganic strong acid cobalt salt is cobalt chloride or cobalt nitrate; the mass volume ratio of the inorganic strong acid zinc salt or inorganic strong acid cobalt salt and the Na4Fe3(PO4)2P2O7 / rGO mixed solution is 10-50 mg:30 mL; the stirring time is 3-7 h; and the calcination process is firstly heating to 300-350°C and keeping warm for 1-3 h; then heating to 550-600°C and keeping warm for 8-10 h.
[0011] In a second aspect, the present invention provides a Tremella-like sodium iron phosphate pyrophosphate composite material prepared by the above method.
[0012] In a third aspect, the present invention also provides the use of the tremella-like sodium iron phosphate pyrophosphate composite material prepared by the above method in a sodium ion battery.
[0013] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: 1. The tremella-like sodium iron phosphate pyrophosphate composite material provided by the technical solution of the present invention comprises a three-dimensional sheet rGO material and a Na4Fe3(PO4)2P2O7 spherical material, wherein the diameter of the Na4Fe3(PO4)2P2O7 spherical material is 2 to 6 microns; the Na4Fe3(PO4)2P2O7 spherical material is embedded in the three-dimensional sheet rGO material to form a tremella-like three-dimensional composite structure; The surface of the three-dimensional sheet rGO material is also uniformly loaded with metal nanocrystals of zinc or cobalt; the Na4Fe3(PO4)2P2O7 spherical material is a micron-sized material formed by the accumulation of nanoparticles. Compared with the prior art, it can not only improve the stability of the material structure, but also facilitate electrolyte infiltration and ion shuttle, thereby accelerating the kinetic reaction; The spherical Na4Fe3(PO4)2P2O7 material is embedded in the three-dimensional sheet rGO material to form a three-dimensional composite structure similar to Tremella fuciformis. Compared with carbon coating and carbon doping, the three-dimensional composite structure similar to Tremella fuciformis connects multiple spherical precursor individuals, and there are more paths for the transfer of ions and electrons at the interfaces of different spheres. It also has a certain volume limiting effect on the spheres embedded therein, which is more conducive to maintaining the stability of the positive electrode material structure and further improving the cycle stability of sodium ion batteries. The electrons on rGO are transferred along the carbon chain. After the metal nanocrystals of zinc or cobalt are loaded, a conductive sub-path in which the carbon chain and the metal nanocrystals intersect each other is formed. The electrons are transferred along the transfer path with the least resistance in the cross-conductive network path, which greatly reduces the resistance of electron transfer. Compared with the carbon source modified material, the metal nanocrystals used in the present invention have higher conductivity and better dispersion uniformity, and can significantly improve the conductivity of the conductive network.
[0014] The technical solution of the present invention uses ultrasound to highly evenly disperse the Na4Fe3(PO4)2P2O7 spherical precursor and GO in water, and reduces GO to rGO through a hydrothermal reaction, ultimately forming a tremella-like three-dimensional composite structure in which the Na4Fe3(PO4)2P2O7 spherical material is embedded in a three-dimensional flaky rGO material, thereby improving the stability of the positive electrode material structure and thereby improving the cycle stability of the sodium ion battery.
[0015] The technical solution of the present invention is to add zinc salt or cobalt salt to the Na4Fe3(PO4)2P2O7 / rGO mixed solution, and the metal salt is evenly dispersed on the Na4Fe3(PO4)2P2O7 / rGO material after being dissolved, and the metal salt is converted into metal nanocrystals by carbon reduction during high-temperature calcination; the metal nanocrystals are evenly deposited on the rGO to form a three-dimensional thin film framework; compared with a single carbon material, not only the amount of carbon introduced is reduced, but also the conductivity of the conductive network is improved.
[0016] The technical solution of the present invention adopts spray drying to prepare Na4Fe3(PO4)2P2O7 precursor. If the flow rate is too fast, the spray droplets are large and a higher temperature is required to dry them, which increases energy consumption. However, if the drying temperature is not reached, the nozzle will be blocked. If the flow rate is too slow, the material preparation efficiency is low, so matching temperature and flow rate are required to carry out the spray drying process. The present invention can make the precursor particle size distribution between 2 and 6 microns by controlling the flow rate and temperature. Na4Fe3(PO4)2P2O7 / rGO is calcined in an Ar-H2 mixed atmosphere. The hydrogen reduction atmosphere can avoid multiple valence states of iron ions, thereby ensuring the purity and specific capacity of the target material.
[0017] 2. The technical solution of the present invention effectively improves the reaction kinetics of Na4Fe3(PO4)2P2O7 and optimizes the rate performance of Na4Fe3(PO4)2P2O7. At a high current density of 50C, it can still release 77.09mAhg -1 At 1C current density, it can still release 83.56 mAh g after 2100 cycles. -1 The cycle attenuation rate is as low as 0.003%, the Coulomb efficiency is as high as 99.97%, and the retention rate is 93.12%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a SEM morphology image of the Na4Fe3(PO4)2P2O7 precursor obtained in Example 1 at an electron microscope magnification of 1540 times; Figure 2 This is a SEM morphology image of the Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) obtained in Example 1 at an electron microscope magnification of 3860 times; Figure 3 This is a SEM morphology of the Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) obtained in Example 1 at an electron microscope magnification of 5060 times; Figure 4 This is the XRD diffraction pattern of the Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) obtained in Example 1; Figure 5 The tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) obtained in Example 1 is used as a positive electrode material in a sodium ion battery, and the rate performance diagram at different current densities; Figure 6 This is a long cycle diagram of the tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) obtained in Example 1 used as a positive electrode material in a sodium ion battery at a current density of 1C. DETAILED DESCRIPTION
[0019] The present invention is further described in detail below in conjunction with the embodiments. The drawings and embodiments of the specification are only used to explain the present invention and do not constitute an improper limitation of the present invention. Example 1
[0020] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.3 mol ferric nitrate, and 0.05 mol citric acid to 500 mL of deionized water and stir to react. -1 The Na4Fe3(PO4)2P2O7 material precursor was obtained by spray drying under the following conditions; (2) 0.2 g Na4Fe3(PO4)2P2O7 material precursor and 10 mg GO were added to 30 mL deionized water and ultrasonically dispersed for 30 min to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution, which was then transferred to a reactor and reacted at 160 °C for 24 h to obtain a Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution; (3) The Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution was transferred to a beaker, 50 mg of zinc nitrate was added thereto and stirred for 5 h. The suspension was evenly stirred to form a suspension, which was then filtered, washed and dried to obtain a composite material precursor. The composite material precursor was calcined in an Ar-H2 atmosphere, first at 300°C for 1 h, and then the temperature was increased to 550°C and calcined for 10 h to obtain a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn).
[0021] The Na4Fe3(PO4)2P2O7 precursor obtained in Example 1 was observed using a scanning electron microscope. Figure 1As shown, the precursor is a spherical material with a particle size distribution of 2~6μm. The final material obtained in Example 1 was observed. The spherical material Na4Fe3(PO4)2P2O7 was embedded in the three-dimensional flaky rGO material to form a Tremella-like three-dimensional composite structure. Compared with carbon coating and carbon doping, the Tremella-like three-dimensional composite structure connects multiple spherical precursor individuals, and there are more pathways for transferring ions and electrons at different spherical interfaces. And there is a certain volume limitation effect on the spheres embedded therein, which is more conducive to maintaining the stability of the positive electrode material structure and further improving the cycle stability of the sodium ion battery. The electrons on rGO are transferred along the carbon chain. After loading the metal nanocrystals, a conductive sub-path in which the carbon chain and the metal nanocrystals intersect with each other is formed. The electrons are transmitted along the transfer path with the least resistance in the cross-conductive network path. The present invention introduces metal nanocrystals with higher conductivity and good dispersion uniformity. The metal nanocrystals and the carbon source cooperate with each other to provide a conductive network with higher conductivity, such as Figure 2 and Figure 3 The powder finally obtained in this example was subjected to XRD diffraction test, and the results are as follows Figure 4 Synthesis of the demonstrated materials. Example 2
[0022] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.29 mol ferric chloride, and 0.05 mol citric acid to 500 mL of deionized water and stir to react. -1 The Na4Fe3(PO4)2P2O7 material precursor was obtained by spray drying under the following conditions; (2) 0.3 g Na4Fe3(PO4)2P2O7 material precursor and 30 mg GO were added to 30 mL deionized water and ultrasonically dispersed for 30 min to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution, which was then transferred to a reactor and reacted at 150 °C for 15 h to finally obtain a Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution; (3) The Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution was transferred to a beaker, 50 mg of cobalt nitrate was added thereto and stirred for 7 h. The suspension was evenly stirred to form a suspension, which was then filtered, washed and dried to obtain a composite material precursor. The composite material precursor was calcined in an Ar-H2 atmosphere, first at 350°C for 3 h, and then at 550°C for 8 h to obtain a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Co). Example 3
[0023] (1) Add 0.4 mol sodium hypophosphite, 0.31 mol ferric nitrate, and 0.03 mol glucose into 500 mL deionized water and stir to react. -1 The Na4Fe3(PO4)2P2O7 material precursor was obtained by spray drying under the following conditions; (2) 0.5 g Na4Fe3(PO4)2P2O7 material precursor and 50 mg GO were added to 30 mL deionized water and ultrasonically dispersed for 30 min to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution, which was then transferred to a reactor and reacted at 180 °C for 20 h to finally obtain a Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution; (3) The Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution was transferred to a beaker, 30 mg of zinc chloride was added thereto, stirred for 3 h, and then filtered, washed, and dried to obtain a composite material precursor; the composite material precursor was calcined in an Ar-H2 atmosphere, first at 300°C for 1 h, then heated to 550°C for 8 h, and finally a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Zn) was obtained. Example 4
[0024] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.3 mol ferric nitrate, and 0.05 mol citric acid to 500 mL of deionized water and stir to react. -1 The Na4Fe3(PO4)2P2O7 material precursor was obtained by spray drying under the following conditions; (2) 0.2 g Na4Fe3(PO4)2P2O7 material precursor and 10 mg GO were added to 30 mL deionized water and ultrasonically dispersed for 30 min to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution, which was then transferred to a reactor and reacted at 160 °C for 24 h to finally obtain a Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution; (3) The Na4Fe3(PO4)2P2O7 precursor / rGO mixed solution was transferred to a beaker, 50 mg of cobalt chloride was added thereto and stirred for 5 h, then stirred evenly to form a suspension, which was filtered, washed and dried to obtain a composite material precursor; the composite material precursor was calcined in an Ar-H2 atmosphere, first at 300°C for 1 h, then heated to 600°C for 10 h, and finally a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO / Co) was obtained. Comparative Example
[0025] (1) Add 0.4 mol sodium dihydrogen phosphate, 0.3 mol ferric nitrate, and 0.05 mol citric acid to 500 mL of deionized water and stir to react. -1 The Na4Fe3(PO4)2P2O7 material precursor was obtained by spray drying under the following conditions; (2) 0.2 g Na4Fe3(PO4)2P2O7 material precursor and 10 mg GO were added to 30 mL deionized water and ultrasonically dispersed for 30 min to form a Na4Fe3(PO4)2P2O7 precursor / GO mixed solution, which was then transferred to a reactor and reacted at 160 °C for 24 h to obtain a suspension, which was then filtered, washed, and dried to obtain a composite material precursor; the composite material precursor was calcined in an Ar-H2 atmosphere, first at 300 °C for 1 h, then heated to 550 °C for 10 h, and finally a Tremella-like sodium iron phosphate pyrophosphate composite material (Na4Fe3(PO4)2P2O7 / rGO) was obtained.
[0026]
[0027] The materials prepared in the examples and comparative examples were used as positive electrodes in sodium ion batteries. From the data in Table 1, it can be seen that the electrochemical performance of the material obtained in Example 1 is the best, proving that this condition is optimal. The specific capacity released by the composite materials loaded with Zn metal nanocrystals obtained in Examples 1 and 3 is higher than that of the composite materials loaded with Co metal nanocrystals in Examples 2 and 4, proving that Zn nanocrystals and rGO synergistically improve conductivity. The electrochemical performance of the material in the comparative example that is not loaded with metal nanocrystals is the worst, proving that the loading of metal nanocrystals is effective. The material structure designed in this patent effectively improves the conductivity of the material and accelerates the reaction kinetics, showing the following performance: Figure 5 The excellent rate performance shown in Figure 1 is that it can still release 77.09 mAh g at a current density of up to 50 C. -1 The Tremella-like structure can better maintain the structural stability of the material. The test results at 1C current density are as follows: Figure 6 As shown, the first cycle discharge capacity is 89.73 mAh g -1 After 2100 cycles, it can still release 83.56 mAh g -1 The cycle attenuation rate is as low as 0.003%, the Coulomb efficiency is as high as 99.97%, and the retention rate is 93.12%.
Claims
1. A method for preparing a Tremella-like sodium iron phosphate pyrophosphate composite material, It is characterized in that The steps include: (1) Dissolve an inorganic salt containing sodium and phosphorus, a chain carbon source and an inorganic strong acid iron salt in deionized water and stir to react, and spray dry the reaction solution to obtain Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 Material precursors; (2) Put Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The material precursor and GO were added into deionized water and ultrasonically dispersed to form Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 Precursor / GO mixed solution; hydrothermal reaction to obtain Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 Precursor / rGO mixed solution; (3) To Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 Inorganic strong acid zinc salt or inorganic strong acid cobalt salt is added to the precursor / rGO mixed solution, stirred evenly to form a suspension, filtered, washed and dried to obtain a composite material precursor; in an Ar-H 2 The composite material precursor is calcined in an atmosphere, and a tremella-like sodium iron phosphate pyrophosphate composite material is obtained after the calcination is completed.
2. The preparation method of the Tremella-like sodium iron pyrophosphate composite material according to claim 1, It is characterized in that In the step (1), the inorganic salt containing sodium and phosphorus is sodium hypophosphite or sodium dihydrogen phosphate; the inorganic strong acid iron salt is ferric nitrate or ferric chloride; the chain carbon source is glucose or citric acid; the molar ratio of the inorganic salt containing sodium and phosphorus, the inorganic strong acid iron salt, and the chain carbon source is 0.4 mol: 0.29-0.31 mol: 0.03-0.05 mol; the spray drying temperature is 110-150°C; and the flow rate is 200-300 mL / h -1 .
3. The preparation method of the Tremella-like sodium iron phosphate pyrophosphate composite material according to claim 1, It is characterized in that In the step (2), Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The mass ratio of the material precursor to GO is 10~20:1; the hydrothermal reaction temperature is 150~180℃; and the hydrothermal reaction time is 15~24h.
4. The preparation method of the Tremella-like sodium iron pyrophosphate composite material according to claim 1, It is characterized in that In the step (3), the inorganic strong acid zinc salt is zinc chloride or zinc nitrate; the inorganic strong acid cobalt salt is cobalt chloride or cobalt nitrate; the inorganic strong acid zinc salt or inorganic strong acid cobalt salt, Na 4 Fe 3 (PO 4 ) 2 P 2 O 7 The mass volume ratio of the / rGO mixed solution is 30~50mg:30 mL; the stirring time is 3~7h; the calcination process is firstly heating to 300~350℃ and keeping warm for 1~3h; then heating to 550~600℃ and keeping warm for 8~10h.
5. A tremella-like sodium iron phosphate pyrophosphate composite material prepared by the method according to any one of claims 1 to 4.
6. Use of the tremella-like sodium iron phosphate pyrophosphate composite material as claimed in claim 5 in a sodium ion battery.
Citation Information
Patent Citations
Hollow spherical Na<4>Fe<3>(PO<4>)<2>P<2>O<7> / C composite positive electrode material and preparation method therefor
CN107069012A
RGO-alpha-Fe2O3 / ZnFe2O4 composite material as well as preparation method and application thereof
CN117783221A
Composite ferric sodium pyrophosphate material and preparation method thereof
CN117945377A
Creating conductivized traces for use in electronic devices
US20120186080A1
Battery electrode and method of making the same
WO2024184368A1
Cited By
High-conductivity three-dimensional carbon nano-wire modified composite phosphate material and preparation method thereof
CN119725481A
Highly conductive three-dimensional carbon nanofilament modified composite phosphate material and preparation method thereof
CN119725481B