Preparation method of phenolic resin-based hard carbon nanospheres with adjustable particle size and carbon structure

Phenolic resin nanospheres were prepared by rapid reaction using phenol source and co-catalyst in aqueous solution and then carbonized under an inert atmosphere. This solved the problem of difficult control of particle size and structure in the prior art, and achieved efficient and low-cost preparation of hard carbon nanospheres, thus improving the electrochemical performance of sodium-ion batteries.

CN118929620AInactive Publication Date: 2024-11-12BEIJING UNIV OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410916456.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies require the use of acid-base catalysts and organic solvents when preparing phenolic resin-based hard carbon microspheres, which makes it difficult to control particle size and structure and is not suitable for large-scale production.

Method used

Phenolic resin nanospheres were prepared by rapid reaction in aqueous solution using a phenolic source and a co-catalyst with autocatalytic function, and then carbonized under an inert atmosphere to prepare hard carbon nanospheres with controllable particle size and tunable structure.

Benefits of technology

This method enables the rapid, simple, and controllable preparation of phenolic resin nanospheres at room temperature, avoiding the use of organic solvents and acid-base catalysts. It improves the interlayer spacing and amorphousness of hard carbon nanospheres, thereby enhancing the cycle stability and rate performance of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929620A_ABST
    Figure CN118929620A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of phenolic resin-based hard carbon nanospheres with adjustable particle sizes and carbon structures. The phenolic resin-based hard carbon nanospheres are mainly applied to a negative electrode material of a sodium-ion battery. According to the method, a phenol source with an autocatalysis function, formaldehyde and a cocatalyst are used for rapidly reacting in an aqueous solution, an acid-base catalyst and an organic solvent are not used, and the phenolic resin nanospheres with uniform particle size and good dispersion can be synthesized at room temperature. And then, carrying out high-temperature carbonization to obtain the hard carbon nanospheres. The cocatalyst regulates the particle size and molecular structure of the phenolic resin nanospheres, enhances the interlayer spacing and amorphous degree of the hard carbon, and improves the electrochemical performance of the hard carbon. The prepared hard carbon nanosphere shows excellent cycling stability and rate capability in the sodium ion battery. The method is simple to operate, low in cost and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a preparation method and application of a water-based phenolic resin-based hard carbon nanosphere material with adjustable particle size and carbon structure. Background Art

[0002] Sodium-ion batteries have good application prospects in large-scale energy storage and are the most promising alternative to lithium-ion batteries. Hard carbon materials are considered to be the preferred negative electrode materials for commercial sodium-ion batteries. Among them, spherical hard carbon materials have attracted much attention due to their advantages such as high stacking density, high coulombic efficiency, high volumetric capacity and high cycle stability. In addition to the spherical structure, spherical hard carbon also needs to have a nanoscale diameter, high amorphousness and large interlayer spacing. These characteristics help to improve the sodium ion storage capacity and rate performance of hard carbon spheres.

[0003] Phenolic resin materials are widely available, low in cost, and have a high residual carbon rate after carbonization. They are one of the main precursors of hard carbon. Phenolic resin is easy to form a spherical structure, and hard carbon balls can be obtained through subsequent carbonization treatment and other processes. Researchers have conducted many studies on phenolic resin-based spherical hard carbon. For example, in the patent "A method for preparing a phenolic resin-based hard carbon microsphere material", phenol and aldehyde synthesize phenolic resin oligomers under the action of an alkaline catalyst, and then spray dry at 120°C to obtain phenolic resin microspheres. In another patent "A phenolic resin-based spherical hard carbon negative electrode material with adjustable architecture for sodium ion batteries and its preparation method", phenol source and aldehyde react at 100°C for 6 to 12 hours under different alkaline catalysts to regulate the structure of phenolic resin microspheres. Zhao et al. used 3-aminophenol and formaldehyde in a water / ethanol system to heat and polymerize at 75°C for 4 hours to prepare highly monodisperse phenolic resin microspheres, and adjusted the particle size from 372 nanometers to 1030 nanometers by controlling the reaction temperature and monomer concentration. However, previous synthesis processes required the use of acid-base catalysts, organic solvents, heating and long reaction times, which posed challenges to large-scale production and made it difficult to precisely control particle size and structure.

[0004] Therefore, it is of great significance to find a method that avoids the use of organic solvents and acid-base catalysts and quickly synthesizes phenolic resin-based hard carbon microspheres with controllable particle size and structure in aqueous solution at room temperature. Summary of the invention

[0005] The present invention aims to provide a rapid synthesis method at room temperature without using acid-base catalysts and organic solvents, which is used for preparing phenolic resin nanospheres and hard carbon nanospheres with controllable diameter and adjustable molecular structure.

[0006] The method of the present invention uses a phenol source, formaldehyde and a co-catalyst with an autocatalytic function to quickly prepare phenolic resin nanospheres in an aqueous solution, and then prepares phenolic resin-based hard carbon nanospheres by carbonization. In the aqueous solution, the phenol source and formaldehyde can undergo a polymerization reaction without the need for an external acid-base catalyst to form a phenolic resin molecular network structure. The co-catalyst is mainly an anionic surfactant containing a carboxylic acid or sulfonic acid group, which can not only regulate the particle size of the phenolic resin nanospheres, but also catalyze the ring-opening reaction of the phenolic resin molecular network, thereby regulating the molecular structure and enhancing the interlayer spacing and amorphousness of the hard carbon. The phenolic resin microspheres prepared by the present invention have good cycle stability and rate performance as a negative electrode material for sodium ion batteries. The entire preparation process is fast, simple, controllable and low-cost.

[0007] The present invention provides the following technical solutions:

[0008] A method for preparing phenolic resin-based hard carbon nanospheres with adjustable particle size and carbon structure comprises the following steps:

[0009] (1) First, a phenol source and a co-catalyst are dissolved in deionized water to prepare a clear solution A; then, a formaldehyde aqueous solution is added to the solution A according to a certain phenol source / formaldehyde molar ratio, reacted at room temperature for a certain time, and phenolic resin nanospheres are obtained after centrifugation, washing, and drying.

[0010] (2) placing the phenolic resin nanospheres obtained in step (1) in an inert gas atmosphere for high-temperature carbonization to obtain hard carbon nanospheres. Preferably, the phenol source in step (1) is one of 3-aminophenol, 3-aminomethylphenol, 3-(methylamino)phenol, 3-(ethylamino)phenol, 3-(acetylamino)phenol, 3-cyclohexylaminophenol, and 3-amino-4-methylphenol.

[0011] Preferably, in step (1), the concentration of the phenol source in solution A is 5 to 36 g / L.

[0012] Preferably, the co-catalyst in step (1) is linoleic acid, ammonium linoleate, sodium linoleate, stearic acid, ammonium stearate, sodium stearate, dodecylbenzenesulfonic acid, ammonium dodecylbenzenesulfonate, sodium dodecylbenzenesulfonate.

[0013] Preferably, in step (1), the concentration of the promoter in solution A is 10 to 50 mg / L. Preferably, in step (1), the molar ratio of phenol source to formaldehyde is 1:2 to 1:6.

[0014] Preferably, the reaction time in step (1) is 5-10 min.

[0015] Preferably, the solvent used for washing in step (1) is deionized water.

[0016] Preferably, the inert gas introduced in step (2) is nitrogen or argon.

[0017] Preferably, the carbonization temperature in step (2) is 1000-1800°C.

[0018] The present invention provides a method for preparing phenolic resin-based hard carbon nanospheres with adjustable particle size and carbon structure. At room temperature, without using catalysts and organic solvents, phenolic resin nanospheres with uniform particle size distribution are synthesized through aqueous solution, and their structure and particle size are regulated by a co-catalyst. The phenolic resin-based hard carbon nanospheres prepared after carbonization are mainly used as high-performance sodium ion battery negative electrode materials. The negative electrode of the sodium ion battery is composed of the following components in mass percentage: 80% phenolic resin-based hard carbon microspheres, 10% acetylene black, and 10% binder. The beneficial effects are as follows: Phenolic resin-based hard carbon nanospheres without adding co-catalysts are used as the negative electrode material of the sodium ion battery. At 30mAg -1 At a current density of 283 mAh g -1 The electrochemical performance of phenolic resin-based hard carbon microspheres was significantly improved after adding the catalyst. -1 At a current density of 323 mAh g -1 The reversible capacity is 5Ag -1 The present invention has the following advantages over the prior art:

[0019] 1. The phenolic resin microspheres prepared by the present invention are uniformly dispersed, have a uniform particle size, and have a high carbonization yield by rapidly reacting with formaldehyde in an aqueous solution without using an acid-base catalyst.

[0020] 2. The present invention is carried out in a pure water system at room temperature without using organic solvents, thus avoiding the uncontrollable defects and environmental problems caused by organic solvents, and the reaction is fast.

[0021] 3. The co-catalyst uses surface tension and catalytic action during the rapid preparation process to control the particle size and structure of the microspheres, thereby achieving controllable preparation of hard carbon microspheres.

[0022] 4. The raw materials used in the present invention are cheap, and while achieving rapid and controllable preparation, the goal of low cost is also achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Attached Figure 1 This is a scanning electron microscope (SEM) image of the phenolic resin-based hard carbon microspheres obtained in Example 1.

[0024] Attached Figure 2 This is a high-resolution transmission electron microscopy (HRTEM) image of the phenolic resin-based hard carbon microspheres obtained in Example 1.

[0025] Attached Figure 3 This is the SEM image of the phenolic resin-based hard carbon microspheres obtained in Example 2.

[0026] Attached Figure 4 This is the SEM image of the phenolic resin-based hard carbon microspheres obtained in Comparative Example 1.

[0027] Attached Figure 5 This is the HRTEM image of the phenolic resin-based hard carbon microspheres obtained in Comparative Example 1.

[0028] Attached Figure 6 This is the SEM image of the phenolic resin-based hard carbon microspheres obtained in Comparative Example 2. DETAILED DESCRIPTION

[0029] The present invention is further explained below by specific examples, but the scope of the present invention is not limited to the following examples. Without departing from the concept of the present invention, various substitutions or changes made according to common technical knowledge and customary means in the art should be included in the scope of the present invention:

[0030] Example 1

[0031] (1) 1.2 g of 3-aminophenol and 1 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution, and the mixture was reacted at room temperature for 10 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0032] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000°C to obtain hard carbon nanospheres. The size of the microspheres after carbonization is 232.4 nm. Figure 1 The interlayer spacing is As attached Figure 2 shown.

[0033] Example 2

[0034] (1) 1.2 g of 3-aminophenol and 1 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution, reacted at room temperature for 8 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0035] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000°C to obtain hard carbon nanospheres. The size of the microspheres after carbonization is 203.2 nm. Figure 3 shown.

[0036] Example 3

[0037] (1) 1.2 g of 3-aminophenol and 1 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 4.8 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:6) was added to the solution, reacted at room temperature for 5 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0038] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0039] Example 4

[0040] (1) 1.2 g of 3-aminophenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0041] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0042] Example 5

[0043] (1) 1.2 g of 3-aminophenol and 5 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0044] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0045] Example 6

[0046] (1) 1.2 g of 3-aminophenol and 5 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0047] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1300° C. to obtain hard carbon nanospheres.

[0048] Example 7

[0049] (1) 1.2 g of 3-aminophenol and 5 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0050] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1500° C. to obtain hard carbon nanospheres.

[0051] Example 8

[0052] (1) 1.2 g of 3-aminomethylphenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution, reacted at room temperature for 5 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0053] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0054] Example 9

[0055] (1) 1.2 g of 3-(methylamino)phenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0056] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0057] Example 10

[0058] (1) 1.2 g of 3-(ethylamino)phenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0059] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0060] Embodiment 11

[0061] (1) 1.2 g of 3-(acetylamino)phenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution, reacted at room temperature for 5 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0062] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1100° C. to obtain hard carbon nanospheres.

[0063] Example 12

[0064] (1) 1.2 g of 3-cyclohexylaminophenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution, reacted at room temperature for 5 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0065] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0066] Example 13

[0067] (1) 1.2 g of 3-amino-4-methylphenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0068] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0069] Embodiment 14

[0070] (1) 1.2 g of 3-aminophenol and 2 mg of linoleic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0071] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0072] Embodiment 15

[0073] (1) 1.2 g of 3-aminophenol and 2 mg of ammonium linoleate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio is 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0074] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0075] Example 16

[0076] (1) 1.2 g of 3-aminophenol and 2 mg of sodium linoleate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0077] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0078] Embodiment 17

[0079] (1) 1.2 g of 3-aminophenol and 2 mg of stearic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0080] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0081] Embodiment 18

[0082] (1) 1.2 g of 3-aminophenol and 2 mg of ammonium stearate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0083] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0084] Embodiment 19

[0085] (1) 1.2 g of 3-aminophenol and 2 mg of sodium stearate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio is 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0086] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0087] Embodiment 20

[0088] (1) 1.2 g of 3-aminophenol and 2 mg of dodecylbenzenesulfonic acid were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0089] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0090] Embodiment 21

[0091] (1) 1.2 g of 3-aminophenol and 2 mg of ammonium dodecylbenzenesulfonate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio is 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0092] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0093] Embodiment 22

[0094] (1) 1.2 g of 3-aminophenol and 2 mg of sodium dodecylbenzene sulfonate were dissolved in deionized water to prepare a clear solution; then 3.2 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:4) was added to the solution. The formaldehyde aqueous solution was added to the solution and reacted at room temperature for 5 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0095] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000° C. to obtain hard carbon nanospheres.

[0096] Comparative Example 1

[0097] (1) 1.2 g of 3-aminophenol was dissolved in deionized water to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution, reacted at room temperature for 10 min, and phenolic resin nanospheres were obtained after centrifugation, washing, and drying.

[0098] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000°C to obtain hard carbon nanospheres. The size of the microspheres after carbonization is 562.2 nm. Figure 4 The interlayer spacing is As attached Figure 5 shown.

[0099] Without the participation of a co-catalyst, the control effect of the surface tension is lost during the reaction process, and the obtained hard carbon microspheres have a larger particle size and a lower degree of cross-linking, resulting in a smaller structural layer spacing of the hard carbon microspheres.

[0100] Comparative Example 2

[0101] (1) 1.2 g of 3-aminophenol was dissolved in ethanol to prepare a clear solution; then 1.6 ml of formaldehyde solution (phenol source / formaldehyde molar ratio was 1:2) was added to the solution, and the mixture was reacted at room temperature for 30 min. After centrifugation, washing, and drying, phenolic resin nanospheres were obtained.

[0102] (2) The phenolic resin nanospheres obtained in step (1) are placed in an inert gas atmosphere and carbonized at 1000°C to obtain hard carbon nanospheres with uneven particle size and defects. Figure 6 shown.

[0103] The presence of ethanol not only causes the phenolic resin microspheres to present an irregular spherical shape, but also remains in the bulk phase of the phenolic resin microspheres, causing uncontrollable internal defects and hindering the polymerization reaction to a certain extent, thereby prolonging the reaction time.

[0104] The following table compares the reaction time, molar ratio of phenol source to aldehyde, resin particle size, particle size of carbon nanoparticles, carbonization temperature, interlayer spacing and electrochemical performance of the phenolic resin microspheres obtained in Examples 1-22 and Comparative Examples 1-2.

[0105]

[0106]

[0107] It can be seen from the data in the table that, in Examples 1-3, as the phenol source / formaldehyde molar ratio increases, the reaction rate accelerates, the particle size decreases, the interlayer spacing increases, and the reversible specific capacity of the battery gradually increases. In Examples 1 and 4-5, as the amount of co-catalyst added increases, the particle size decreases, the interlayer spacing increases, and the reversible specific capacity of the battery also gradually increases. In Examples 5-7, as the carbonization temperature increases, the diameter of the obtained carbon nano-microspheres increases, the interlayer spacing decreases, and the reversible capacity of the battery decreases. In Examples 8-22, by changing the phenol source and the co-catalyst, the particle size and interlayer spacing are controlled, which conforms to the rule that the larger the particle size, the smaller the interlayer spacing, and the lower the reversible capacity of the battery, which is due to the surface tension and catalytic effect of the co-catalyst during the reaction.

[0108] In Comparative Example 1, no co-catalyst is added, and the reaction time is extended to 15 minutes. The obtained phenolic resin microspheres and carbon nano-microspheres have large particle sizes, small interlayer spacing, and low reversible capacity of the battery. In Comparative Example 2, ethanol is used as a solvent, and the reaction time is extended to 30 minutes. The obtained phenolic resin microspheres and carbon microspheres have large particle sizes and uneven distribution, and there are defects. This is because the organic solvent remains in the bulk phase of the phenolic resin microspheres, resulting in uncontrollable internal defects, and hinders the polymerization reaction to a certain extent, thereby prolonging the reaction time.

Claims

1. A method for preparing phenolic resin-based hard carbon nanospheres with adjustable particle size and carbon structure, characterized in that: The method comprises the following steps: 1) Firstly, a phenol source and a co-catalyst are dissolved in water to prepare a clear solution A; then, a formaldehyde aqueous solution is added to the solution A according to a certain phenol source / formaldehyde molar ratio, reacted at room temperature for a certain time, and phenolic resin nanospheres are obtained after centrifugation, washing and drying. 2) The phenolic resin nanospheres obtained in step 1) are placed in an inert gas atmosphere for high-temperature carbonization to obtain hard carbon nanospheres.

2. The preparation method according to claim 1, characterized in that The phenol source in step 1) is one of 3-aminophenol, 3-aminomethylphenol, 3-(methylamino)phenol, 3-(ethylamino)phenol, 3-(acetylamino)phenol, 3-cyclohexylaminophenol and 3-amino-4-methylphenol.

3. The preparation method according to claim 1, characterized in that The concentration of the phenol source in the solution A in step 1) is 5-36 g / L.

4. The preparation method according to claim 1, characterized in that The co-catalyst in step 1) is linoleic acid, ammonium linoleate, sodium linoleate, stearic acid, ammonium stearate, sodium stearate, dodecylbenzenesulfonic acid, ammonium dodecylbenzenesulfonate, sodium dodecylbenzenesulfonate.

5. The preparation method according to claim 1, characterized in that The concentration of the co-catalyst in the solution A in step 1) is 10-50 mg / L.

6. The preparation method according to claim 1, characterized in that The molar ratio of phenol source to formaldehyde in step 1) is 1:2 to 1:

4.

7. The preparation method according to claim 1, characterized in that The reaction time in step 1) is 5-10 min.

8. The preparation method according to claim 1, characterized in that The inert gas in step 2) is nitrogen or argon.

9. The preparation method according to claim 1, characterized in that The carbonization temperature in step 2) is 1000-1800°C.

Citation Information

Patent Citations

  • Autocatalysis preparation method of copolymer benzoxazine-resin polymer sphere and autocatalysis preparation method of resin-based carbon sphere

    CN105273188A

  • Resin-based hard carbon microspheres and preparation method thereof

    CN118164468A