Graphitized carbon material and preparation method thereof

By adding carbon-based polymers to the surface of graphene materials and performing defect treatment and/or heteroatom treatment, the problem of insufficient performance of thin-film carbon materials in the prior art has been solved, and a graphitized layer distribution with high orientation degree under low energy consumption has been achieved, which improves the thermal conductivity, electrical conductivity and vibration resistance of the material.

CN118929652AActive Publication Date: 2024-11-12THE NAT CENT FOR NANOSCI & TECH NCNST OF CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411113981.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare highly oriented thin-film carbon materials with low energy consumption, resulting in insufficient thermal conductivity, electrical conductivity, and vibration resistance.

Method used

By adding carbon-based polymers to the surface of graphene materials and performing defect treatment and/or heteroatom treatment on graphene catalysis, the uniform distribution of graphitized layers is promoted and the graphitization temperature is reduced.

Benefits of technology

The mechanical, thermal, and electrical properties of thin-film carbon materials were significantly improved with lower energy consumption, and a graphitized layer distribution with high orientation was achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929652A_ABST
    Figure CN118929652A_ABST
Patent Text Reader

Abstract

The invention provides a graphitized carbon material and a preparation method thereof, and the preparation method comprises the following steps: (1) adding a carbon-based polymer on the surface of a graphene material to obtain a composite film containing a graphene layer and a polymer layer; and (2) carrying out graphitization treatment on the composite film obtained in the step (1) to obtain the graphitized carbon material, the graphene material comprises at least one of untreated graphene and graphene subjected to defect treatment and / or heteroatom treatment. According to the preparation method provided by the invention, by introducing at least one of untreated graphene and graphene subjected to defect treatment and / or heteroatom treatment, graphitization of the carbon-based polymer can be promoted, and catalytic graphitization is performed on the polymer layer from inside to outside and / or from outside to inside, so that the graphitized layer is uniformly distributed in the whole carbon material; the carbon material has excellent thermal properties, mechanical properties and electrical properties, and the graphitization treatment temperature can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a graphitized carbon material and a preparation method thereof. Background Art

[0002] As microelectronic devices develop towards miniaturization and high-density integration, and signal transmission develops towards high frequency and high speed, the heat dissipation problem of electronic devices is becoming more and more important. It is reported that the heat dissipation of electronic devices in 5G is 3 times higher than that in 4G. Therefore, the development of efficient thermal conductive materials is essential for high-power electronic devices and portable devices. Thin-film carbon materials are widely used in various electronic devices due to their high thermal conductivity, electrical conductivity, mechanical strength and modulus. In addition, compared with metal materials such as copper or aluminum, thin-film carbon materials have lighter weight and are considered to be very promising thermal conductive materials. The increase in the degree of graphitization is conducive to improving the thermal conductivity, electrical conductivity, and vibration resistance of thin-film carbon materials. Therefore, the preparation of highly oriented thin-film carbon materials is an important research direction.

[0003] Template methods (including epitaxial growth on a crystal substrate or seed crystal) are often used to prepare ordered materials, but there are few studies on the preparation of high-quality thin-film carbon materials. At present, the synthesis of thin-film carbon materials usually requires a combination of high temperature and high pressure (highly oriented pyrolytic graphite, HOPG). For example, CN112813496A discloses a method for preparing highly oriented pyrolytic graphite, which comprises: first immersing the graphite substrate in a pretreatment solution, taking it out and drying it, and then using a chemical deposition method to pass methane and nitrogen to obtain a pyrolytic graphite plate; when the pyrolytic graphite plate is cooled to 700-750°C, it is placed in a magnetic field and taken out when the temperature drops to 100°C; the pyrolytic graphite plate treated with the magnetic field is taken out and placed in a high-pressure and high-temperature furnace, and an inert gas is passed in for heat treatment. The invention prepares pyrolytic graphite by pretreating the graphite substrate and using chemical vapor deposition. The preparation method improves the orientation of pyrolytic graphite, but the pyrolysis temperature is high and the energy consumption is large.

[0004] Using chemical conversion methods to promote the evolution of the microstructure of carbon materials has become an important strategy for preparing high-quality thin-film carbon materials. The key lies in finding suitable catalysts and thin-film material forming methods.

[0005] For example, CN107601491A discloses a method for preparing three-dimensional graphitized carbon, comprising the following steps: mixing a water-soluble porous polymer and a catalyst in water, drying after the reaction, to obtain a first product; mixing the first product with KOH in an organic solvent, drying after the reaction, to obtain a second product; and sequentially heating and acid washing the second product to obtain three-dimensional graphitized carbon. The graphitized carbon material prepared by the above method is used to prepare positive electrode active materials and negative electrode active materials, improve the energy density and power density of lithium ion capacitors, have good cycle performance, and high operating voltage. However, the orientation degree of the graphitized carbon material is poor.

[0006] Therefore, it is an urgent problem to be solved in this field to find a graphitization catalyst suitable for the formation of thin-film carbon materials and develop a suitable catalytic graphitization method to achieve the preparation of high-quality graphitized films on a macro scale and obtain thin-film carbon materials with greatly improved thermal conductivity and mechanical properties at low energy consumption. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a graphitized carbon material and a method for preparing the same. The preparation method can catalyze graphitization of a carbon-based polymer from the inside to the outside and / or from the outside to the inside by introducing at least one of untreated graphene, defect-treated and / or heteroatom-treated graphene, so that the graphitized layer is evenly distributed throughout the carbon material, thereby improving the mechanical, thermal and electrical properties of the thin film carbon material at a lower energy consumption.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a graphitized carbon material, the preparation method comprising the following steps:

[0010] (1) adding a carbon-based polymer to the surface of a graphene material to obtain a composite film comprising a graphene layer and a polymer layer;

[0011] (2) The composite film obtained in step (1) is graphitized to obtain the graphitized carbon material; the graphene material comprises at least one of untreated graphene and defect-treated and / or heteroatom-treated graphene.

[0012] In the present invention, the preparation method can promote the graphitization of carbon-based polymers by introducing at least one of untreated graphene, defect-treated and / or heteroatom-treated graphene, and catalytically graphitize the polymer layer from the inside to the outside and / or from the outside to the inside, so that the graphitized layer is evenly distributed in the entire carbon material, so that the carbon material has excellent thermal properties, mechanical properties and electrical properties, and the graphitization treatment temperature can be reduced.

[0013] Preferably, the graphene material includes any one of CVD graphene, graphene oxide or exfoliated graphene, or a combination of at least two thereof, preferably CVD graphene and / or graphene oxide.

[0014] In the present invention, the CVD graphene refers to a graphene material grown on a substrate surface by chemical vapor deposition; the graphene oxide and the graphene obtained by exfoliation are formed into a film on a substrate surface in the form of a solution.

[0015] Preferably, the substrate comprises a metal substrate or a non-metal substrate.

[0016] Preferably, the material of the metal substrate includes any one of copper, iron, cobalt, nickel or platinum, or a combination of at least two metals, preferably copper.

[0017] Preferably, the material of the non-metal substrate includes silicon oxide and mica flakes.

[0018] CVD graphene is more preferred in the present invention. CVD graphene can increase the orientation of graphitized carbon in carbon materials, so that carbon-based polymers are orderly oriented from the inside to the outside and / or from the outside to the inside, and reduce their disordered arrangement; and CVD graphene treated with defects and heteroatoms can further increase the degree of orderly orientation of graphitized carbon and improve the mechanical, thermal and electrical properties of carbon materials; the use of small-sheet graphene, such as graphene oxide and graphene obtained by exfoliation, can also promote the graphitization of carbon-based polymers, but the lattice arrangement of the obtained graphitized carbon is relatively disordered, resulting in the mechanical, thermal and electrical properties of the carbon material being slightly worse than those of the graphitized carbon material obtained by CVD graphene catalysis. However, graphene oxide and graphene obtained by exfoliation have the advantages of low cost and convenient processing, and also have practical application value.

[0019] Preferably, the defect treatment and / or heteroatom treatment comprises any one of chemical treatment, plasma treatment or ozone treatment or a combination of at least two thereof, preferably ozone treatment.

[0020] In the present invention, chemical treatment can increase the heteroatom functional groups and defect levels on the graphene surface; plasma treatment can form defects in the graphene structure; ozone treatment can form defects in the graphene structure and achieve oxygen doping for chemical modification.

[0021] Preferably, the chemical treatment method includes any one of a hydrothermal method, a pyrolysis method or a solution method, or a combination of at least two of them.

[0022] Preferably, the chemical treatment reagent includes any one of poly(oxypropylene)diamine, H2O2, NH3, urea or xenon difluoride, or a combination of at least two thereof.

[0023] Preferably, the plasma gas of the plasma treatment includes any one of hydrogen, nitrogen, oxygen or argon, or a combination of at least two of them.

[0024] Preferably, the plasma treatment time is 1 to 300 s, for example, it can be 1s, 2s, 4s, 6s, 8s, 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s, 70s, 80s, 90s, 100s, 120s, 140s, 160s, 180s, 200s, 220s, 240s, 260s, 280s, 300s, etc., and more preferably 10 to 50s.

[0025] Preferably, the power of the plasma treatment is 10-50 W, for example, it can be 10 W, 12 W, 14 W, 16 W, 18 W, 20 W, 22 W, 24 W, 26 W, 28 W, 30 W, 34 W, 38 W, 40 W, 42 W, 44 W, 46 W, 48 W, 50 W, etc.

[0026] Preferably, the ozone treatment equipment is an ultraviolet ozone cleaning machine.

[0027] Preferably, the ozone treatment time is 1 to 15 min, for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, etc., preferably 5 to 10 min.

[0028] Preferably, the thickness of the graphene layer in step (1) is 0.1 to 10 nm, for example, it can be 0.1 nm, 0.2 nm, 0.25 nm, 0.3 nm, 0.32 nm, 0.34 nm, 0.36 nm, 0.38 nm, 0.4 nm, 0.8 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 9.5 nm, 10 nm, etc., preferably 0.3 to 1.0 nm.

[0029] Preferably, the carbon-based polymer includes any one or a combination of at least two of polyacrylonitrile, polymethyl methacrylate, polyimide, polycarbonate, polyarylacetylene, polydivinylbenzene or polyvinyltriphenylethynylsilane, preferably polyacrylonitrile.

[0030] Preferably, the adding method in step (1) includes at least one of coating, solid-state lamination or liquid-phase mixing, and coating is more preferred.

[0031] Preferably, the carbon-based polymer is applied in the form of a carbon-based polymer dispersion.

[0032] Preferably, the solvent of the carbon-based polymer dispersion includes N,N-dimethylformamide.

[0033] Preferably, the solid content of the carbon-based polymer dispersion is 1.0-10%, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0034] Preferably, the coating method comprises spin coating.

[0035] Preferably, the spin coating device is a centrifugal coater.

[0036] Preferably, the coating rotation speed is 1000-8000 r / min, for example, it can be 1000 r / min, 1500 r / min, 2000 r / min, 3000 r / min, 4000 r / min, 5000 r / min, 6000 r / min, 7000 r / min, 8000 r / min, etc.

[0037] Preferably, the coating time is 10 to 60 seconds, for example, 10 seconds, 20 seconds, 30 seconds, 40 seconds, 50 seconds, 55 seconds, 60 seconds, etc.

[0038] Preferably, the thickness of the polymer layer is 300-400 nm, for example, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm, etc.

[0039] Preferably, after obtaining the composite film in step (1), the method further comprises the step of removing the graphene material substrate.

[0040] Preferably, the method of removing the graphene material substrate includes removing it by solution etching.

[0041] Preferably, the solute of the etching solution includes any one of ammonium persulfate, sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, ferric chloride or ferric nitrate, or a combination of at least two thereof.

[0042] Preferably, the concentration of the etching solution is 0.1-1 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, etc.

[0043] Preferably, the equipment for graphitization treatment in step (2) includes a heating furnace.

[0044] Preferably, step (2) further includes a step of preheating the composite film before the graphitization treatment.

[0045] Preferably, the preheating temperature is 200-300°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, etc.

[0046] Preferably, the preheating time is 1 to 4 hours, for example, it can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, etc.

[0047] Preferably, the preheating is performed in an air atmosphere.

[0048] Preferably, the temperature of the graphitization treatment in step (2) is 1000-3000°C, for example, it can be 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, 1800°C, 2000°C, 2200°C, 2400°C, 2600°C, 2800°C, 3000°C, etc.

[0049] Preferably, the time of the graphitization treatment in step (2) is 0.1 to 2 h, for example, it can be 0.1 h, 0.2 h, 0.4 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, etc.

[0050] Preferably, the atmosphere for the graphitization treatment in step (2) is argon and / or hydrogen.

[0051] Preferably, the heating rate and cooling rate of the graphitization treatment in step (2) are independently 4 to 10°C / min, for example, 4°C / min, 4.2°C / min, 4.4°C / min, 4.8°C / min, 5°C / min, 5.2°C / min, 5.4°C / min, 5.8°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min, 9.5°C / min, 10°C / min, etc.

[0052] Preferably, the pressure of the graphitization treatment in step (2) is 101.325 kPa.

[0053] Preferably, the preparation method comprises the following steps:

[0054] (1) coating a carbon-based polymer on the surface of a graphene material to obtain a composite film comprising a graphene layer with a thickness of 0.1 to 10 nm and a polymer layer with a thickness of 300 to 400 nm;

[0055] (2) graphitizing the composite film obtained in step (1) at a temperature of 1000 to 3000° C. for a time of 0.1 to 2 h to obtain the graphitized carbon material;

[0056] The graphene material includes at least one of untreated graphene and defect-treated and / or heteroatom-treated graphene.

[0057] In a second aspect, the present invention provides a graphitized carbon material, which is prepared by the preparation method described in the first aspect.

[0058] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] The preparation method of the graphitized carbon material provided by the present invention comprises coating a carbon-based polymer on the surface of a graphene material and then performing a graphitization treatment. The graphene material serves as a catalyst for graphitization of the carbon-based polymer and can graphitize the carbon-based polymer layer from the inside to the outside and / or from the outside to the inside, so that the graphitized layer is evenly distributed in the entire thin film carbon material; and the orientation of the graphitized carbon layer is similar to that of the graphene layer, so that the mechanical, thermal and electrical properties of the obtained carbon material are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 The Raman spectrum of the graphitized carbon material obtained by the preparation method of the graphitized carbon material provided in Examples 1 to 6 and Comparative Example 1 of the present invention;

[0062] Figure 2 This is a transmission electron microscope image of a graphitized carbon material obtained by the method for preparing a graphitized carbon material provided in Example 7 of the present invention;

[0063] in, Figure 2 a is a transmission electron microscope image of the cross section of graphitized carbon material; Figure 2 b is a transmission electron microscope image of the cross section of graphitized carbon material at high resolution;

[0064] Figure 3 This is a transmission electron microscope image of a graphitized carbon material obtained by the method for preparing a graphitized carbon material provided in Comparative Example 2 of the present invention;

[0065] in, Figure 3 a is a transmission electron microscope image of the cross section of graphitized carbon material; Figure 3 b is a transmission electron microscope image of the cross section of graphitized carbon material at high resolution. DETAILED DESCRIPTION

[0066] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0067] In the present invention, the materials used in all embodiments and comparative examples are as follows:

[0068] Polyacrylonitrile: Polyacrylonitrile was purchased from Shanghai Dibo Biotechnology Co., Ltd., AR grade;

[0069] CVD graphene: Graphene Co., Ltd.;

[0070] Graphene oxide: Hangzhou Gaoxun Technology Co., Ltd.

[0071] Example 1

[0072] This embodiment provides a method for preparing a graphitized carbon material, the preparation method comprising the following steps:

[0073] (1) After a single-layer CVD graphene film (the substrate is a copper substrate) is subjected to ozone treatment in an ultraviolet ozone cleaning machine for 10 minutes, a polyacrylonitrile dispersion (solid content 2%, solvent is N,N-dimethylformamide) is spin-coated on the surface of the single-layer CVD graphene film after the ozone treatment using a centrifugal coating machine, the rotation speed is 3000 r / min, the coating time is 30 seconds, and after drying, the copper substrate is etched and removed using an ammonium persulfate solution with a concentration of 0.5 mol / L to obtain a composite film comprising a graphene layer and a polyacrylonitrile layer;

[0074] (2) The composite film obtained in step (1) is scooped up using a SiO2 / Si substrate, placed in a tubular furnace and heated to 250°C in air, kept warm for 2 hours, then heated to 1500°C at a heating rate of 5°C / min in 50sccm argon, kept warm for 30 minutes, and finally cooled to room temperature in the tubular furnace at a cooling rate of 5°C / min at the same gas flow rate to obtain the graphitized carbon material.

[0075] The structure of the graphitized carbon material obtained in Example 1 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus), and the results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 1 D / I G The value of is approximately 0.552.

[0076] Example 2

[0077] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 1 only in that the time for ozone treatment in step (1) is 5 minutes, and the other steps and parameters are the same as those in Embodiment 1.

[0078] The structure of the graphitized carbon material obtained in Example 2 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus), and the results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 2 D / I G The value of is approximately 0.697.

[0079] Example 3

[0080] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 1 only in that the ozone treatment in step (1) is replaced by argon plasma treatment, the power of the argon plasma treatment is 50 W, and the time is 20 s. The other steps and parameters are the same as those in Embodiment 1.

[0081] The structure of the graphitized carbon material obtained in Example 3 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus). The results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 3 D / I G The value of is approximately 0.754.

[0082] Example 4

[0083] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 3 only in that the time of the argon plasma treatment in step (1) is 50 seconds, and the other steps and parameters are the same as those in Embodiment 3.

[0084] The structure of the graphitized carbon material obtained in Example 4 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus). The results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 4 D / I G The value of is approximately 0.750.

[0085] Example 5

[0086] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 1 only in that the ozone treatment in step (1) is replaced by oxygen plasma treatment, the power of the oxygen plasma treatment is 10 W, and the time is 10 s. The other steps and parameters are the same as those in Embodiment 1.

[0087] The structure of the graphitized carbon material obtained in Example 5 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus). The results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 5 D / I G The value of is approximately 0.763.

[0088] Example 6

[0089] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 1 only in that the graphene material in step (1) is not subjected to defect treatment and / or heteroatom treatment, that is, is not subjected to ozone treatment, and the other steps and parameters are the same as those in Embodiment 1.

[0090] The structure of the graphitized carbon material obtained in Example 6 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus). The results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in Example 6 D / I G The value of is approximately 0.762.

[0091] Example 7

[0092] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 6 only in that the temperature is raised to 1000° C. in argon gas in step (2), and the other steps and parameters are the same as those in Embodiment 6.

[0093] The cross-sectional morphology of the graphitized carbon material obtained in Example 7 was characterized by transmission electron microscopy (TEM, instrument model: Tecnai G2 F20 U-TWIN). The results are as follows: Figure 2 As shown, Figure 2 a is the transmission electron microscope image of the cross section of graphitized carbon material. Figure 2 b is a transmission electron microscope image of the cross section of graphitized carbon material at high resolution; Figure 2 a and Figure 2 b It can be seen that lattice fringes appear in the carbon layer near graphene, and these lattice fringes do not completely belong to the original graphene. It can be seen that graphene material can lower the graphitization temperature of the material, so that graphitization can begin at low temperature, that is, 1000°C, which changes the structure of the material and improves its performance.

[0094] Example 8

[0095] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 1 only in that the time of ozone treatment in step (1) is 15 minutes, and the other steps and parameters are the same as those in Embodiment 1.

[0096] Example 9

[0097] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 3 only in that the time of argon plasma treatment in step (1) is 80 seconds, and the other steps and parameters are the same as those in Embodiment 3.

[0098] Example 10

[0099] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 3 only in that the power of the argon plasma treatment in step (1) is 80 W, and the other steps and parameters are the same as those in Embodiment 3.

[0100] Embodiment 11

[0101] This embodiment provides a method for preparing a graphitized carbon material, which differs from Embodiment 6 only in that in step (1), the single-layer CVD graphene film is replaced by a graphene oxide film of the same thickness, and the other steps and parameters are the same as those in Embodiment 6; the graphene oxide film is obtained by coating a graphene oxide aqueous solution onto a copper substrate and drying it.

[0102] Comparative Example 1

[0103] This comparative example provides a method for preparing a graphitized carbon material, which differs from Example 1 only in that in step (1), the polyacrylonitrile dispersion is directly spin-coated on the surface of the copper substrate, and the other steps and parameters are the same as those in Example 1.

[0104] The structure of the graphitized carbon material obtained in Comparative Example 1 was characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus). The results are as follows: Figure 1 As shown, the graphitized carbon material I obtained by the preparation method provided in the comparative example D / I G About 0.942.

[0105] Comparative Example 2

[0106] This comparative example provides a method for preparing a graphitized carbon material, which differs from comparative example 1 only in that the temperature is raised to 1000° C. in argon in step (2), and the other steps and parameters are the same as those in comparative example 1.

[0107] The cross-sectional morphology of the graphitized carbon material obtained in Comparative Example 2 was characterized by TEM. Figure 3 As shown, Figure 3a is a transmission electron microscope image of the cross section of graphitized carbon material; Figure 3 b is a transmission electron microscope image of the cross section of graphitized carbon material at high resolution. Figure 3 It can be seen from a and 3b that the contrast is uniform throughout the film, and there are no detectable lattice fringes. It can be seen that when no graphene material is added, at 1000°C, the temperature is too low and the material cannot begin to graphitize, and there is no obvious change in structure and performance.

[0108] Performance Testing

[0109] (1)I D / I G :The structures of the graphitized carbon materials obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were characterized by Raman spectroscopy (Raman, instrument model: Renishaw inVia plus); the D peak intensity (1300 cm -1 Nearby, I D ) and G peak intensity (1580cm -1 Nearby, I G ) ratio, I D / I G The smaller it is, the higher the degree of graphitization, the better the orientation, and the better the mechanical, thermal and electrical properties of the graphitized carbon material.

[0110] (2) Electrical properties: In the present invention, the thickness of the graphitized carbon material is 350±10 nm, and the resistivity of the graphitized carbon material is measured by a four-probe method.

[0111] The specific test results are shown in Table 1:

[0112] Table 1

[0113]

[0114]

[0115] As can be seen from the above table, the preparation method of the graphitized carbon material provided by the present invention can catalyze graphitization of the carbon-based polymer from the inside to the outside or from the outside to the inside by introducing at least one of untreated graphene, defect-treated and / or heteroatom-treated graphene, so that the graphitized layer is evenly distributed in the entire carbon material, and the mechanical, thermal and electrical properties of the thin film carbon material are improved at a lower energy consumption; the graphitized carbon material obtained by the preparation method has an I D / I G The resistivity of the graphitized carbon material is 2.2 to 5.7 Ω·cm, and more preferably 2.2 to 3.8 Ω·cm.

[0116] It can be seen from the comparison between Example 1 and Example 8 that when the ozone treatment time is not within a specific range, the I D / I G Increase, the resistivity increases; from the comparison of Example 3 with Examples 9 to 10, it can be seen that when the plasma treatment time or power is not within a specific range, the I D / I G Increases, and the resistivity increases; It can be seen from the comparison between Example 6 and Example 11 that compared with graphene oxide, the carbon material prepared by CVD graphene has better performance.

[0117] It can be seen from the comparison between Example 1 and Comparative Example 1 that when no graphene material is added in the preparation method, the obtained carbon material has poor performance.

[0118] By comparing Example 7 with Comparative Example 2, it can be seen that when graphene material is added to the preparation method, graphitization can begin when the temperature of the graphitization treatment is low, and the resistivity is low; while when no graphene material is added, the structure of the material does not change significantly when the temperature is low, and the resistivity is high. It can be seen that the preparation method provided in the present application can reduce the graphitization treatment temperature.

[0119] In summary, in the method for preparing graphitized carbon materials provided by the present invention, untreated graphene, defect-treated and / or heteroatom-treated graphene have good low-temperature catalytic effect on the formation of graphite structure in polymer; compared with perfect graphene, various defect-treated and / or heteroatom-treated graphene make the I of the composite film D / I G The value decreases; the defective graphene treated with ozone has the most obvious promoting effect on the carbonization process of the polymer, and this promoting effect is further deepened with the increase of defects in the graphene.

[0120] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a graphitized carbon material, characterized in that: The preparation method comprises the following steps: (1) adding a carbon-based polymer to the surface of a graphene material to obtain a composite film comprising a graphene layer and a polymer layer; (2) graphitizing the composite film obtained in step (1) to obtain the graphitized carbon material; The graphene material includes at least one of untreated graphene and defect-treated and / or heteroatom-treated graphene.

2. The preparation method according to claim 1, characterized in that: The graphene material includes any one of CVD graphene, graphene oxide or exfoliated graphene or a combination of at least two thereof, preferably CVD graphene and / or graphene oxide.

3. The preparation method according to claim 1 or 2, characterized in that: The defect treatment and / or heteroatom treatment comprises any one of chemical treatment, plasma treatment or ozone treatment or a combination of at least two thereof, preferably ozone treatment; Preferably, the chemical treatment method includes any one of a hydrothermal method, a pyrolysis method or a solution method, or a combination of at least two thereof; Preferably, the chemical treatment reagent includes any one of poly(oxypropylene)diamine, H2O2, NH3, urea or xenon difluoride, or a combination of at least two thereof.

4. The preparation method according to claim 3, characterized in that: The plasma gas for the plasma treatment includes any one of hydrogen, nitrogen, oxygen or argon, or a combination of at least two of them; Preferably, the plasma treatment time is 1 to 300 s, more preferably 10 to 50 s; Preferably, the power of the plasma treatment is 10-50W.

5. The preparation method according to claim 3, characterized in that: The ozone treatment equipment is an ultraviolet ozone cleaning machine; Preferably, the ozone treatment time is 1 to 15 minutes, preferably 5 to 10 minutes; Preferably, the thickness of the graphene layer in step (1) is 0.1 to 10 nm, preferably 0.3 to 1.0 nm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The carbon-based polymer includes any one or a combination of at least two of polyacrylonitrile, polymethyl methacrylate, polyimide, polycarbonate, polyarylacetylene, polydivinylbenzene or polyvinyltriphenylethynylsilane, preferably polyacrylonitrile; Preferably, the method of adding in step (1) includes at least one of coating, solid-state lamination or liquid-phase mixing, and coating is more preferred; Preferably, the carbon-based polymer is applied in the form of a carbon-based polymer dispersion; Preferably, the solvent of the carbon-based polymer dispersion includes N,N-dimethylformamide; Preferably, the solid content of the carbon-based polymer dispersion is 1.0 to 10%; Preferably, the coating method comprises spin coating; Preferably, the coating rotation speed is 1000-8000 r / min; Preferably, the coating time is 10 to 60 seconds; Preferably, the thickness of the polymer layer is 300-400 nm.

7. The preparation method according to any one of claims 1 to 6, characterized in that: After obtaining the composite film in step (1), the method further comprises the step of removing the graphene material substrate; Preferably, the method of removing the graphene material substrate comprises removing by solution etching; Preferably, the solute of the etching solution includes any one of ammonium persulfate, sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, ferric chloride or ferric nitrate, or a combination of at least two thereof; Preferably, the concentration of the etching solution is 0.1-1 mol / L.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The temperature of the graphitization treatment in step (2) is 1000-3000° C. Preferably, the graphitization treatment time in step (2) is 0.1 to 2 hours; Preferably, the atmosphere of the graphitization treatment in step (2) is argon and / or hydrogen; Preferably, the heating rate and cooling rate of the graphitization treatment in step (2) are independently 4 to 10°C / min; Preferably, the pressure of the graphitization treatment in step (2) is 101.325 kPa.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (1) adding a carbon-based polymer to the surface of a graphene material to obtain a composite film comprising a graphene layer with a thickness of 0.1 to 10 nm and a polymer layer with a thickness of 300 to 400 nm; (2) graphitizing the composite film obtained in step (1) at a temperature of 1000 to 3000° C. for a time of 0.1 to 2 h to obtain the graphitized carbon material; The graphene material includes at least one of untreated graphene and defect-treated and / or heteroatom-treated graphene.

10. A graphitized carbon material, characterized in that: The graphitized carbon material is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of graphene / substrate composite conducting material

    CN104191803A

  • Preparation method of independent self-supporting artificial nano-graphite film

    CN111547716A

  • Defect-state single-layer graphene film as well as preparation method and application thereof

    CN113003568A

  • Preparation method of graphene heat-conducting thick film

    CN113896535A