Magneli phase V6O11 piezoelectric catalyst as well as preparation method and application thereof
The V6O11 nanosheets prepared by the low-temperature hydrothermal method exhibited high catalytic activity under both dark and full-spectrum conditions, solving the problems of complex V6O11 preparation and insufficient catalytic efficiency under dark conditions in existing technologies, and achieving efficient degradation and stability of organic pollutants.
Patent Information
- Application Number
- CN202411093501.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing methods for preparing Magnéli phase V6O11 are complex and dangerous, making them difficult to apply widely in the field of photocatalysis, especially due to insufficient catalytic efficiency under dark conditions.
Using NH4VO3 and VO2 as raw materials and isopropanol and water as solvents, V6O11 nanosheets with a loofah-like structure were prepared at low temperature via a hydrothermal method. Combined with mechanical stress perturbation to form a piezoelectric field, a catalytic reaction was achieved under dark conditions.
The prepared V6O11 material exhibits excellent catalytic activity under both dark and full-spectrum conditions, enabling rapid degradation of organic pollutants. It also demonstrates good cycle stability and photothermal effect, thereby improving the degradation efficiency of both dark catalysis and photocatalysis.
Smart Images

Figure HDA0004987219670000011 
Figure HDA0004987219670000012 
Figure HDA0004987219670000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage piezoelectric dark catalysis and photothermal energy storage piezoelectric catalytic materials and preparation technology, specifically a Magnéli phase V6O 11 Piezoelectric catalyst and its preparation method and application. Background Art
[0002] V6O 11 It is a compound of transition metals that is special because of its ability to form variable valence compounds. Its generalized formula is V n O 2n-1 (n = 3, 6, 9), also known as the Magnéli phase series. The crystal structure of members of this series represents dense hexagonal packing of oxygen ions. V6O 11 The crystal structure is a triclinic system with a P-1(2) space group. Some of the octahedral cavities in the structure are filled with V 3+ and V 4+ Ions fill in, forming VO2 rutile blocks, which are restricted by so-called crystal shear planes and form associations with V2O3. Non-stoichiometric V6O 11 It undergoes a metal-insulator transition accompanied by a conductivity transition of several orders of magnitude.
[0003] V6O 11 V in the crystal 3+ and V 4+ The ratio is 1:2, that is, V 3+ The number is V 4+ According to their ionic radius, during the metal-insulator transition, all V 3+ and half of V 4+ The ions are located at both odd and even sites. The other half of V 4+ The ions will be evenly distributed on the remaining odd and even chains. The arrangement of the chains of equal valence and the packing of the chains themselves make V6O 11 It has a certain degree of arbitrariness, which can adjust the remaining electron exchange between individual vanadium ions, so that V6O 11 Hopping conduction shunting, after which a relatively large number of free carriers remain, which can be 3+ and V 4+ There is a virtual exchange between ions. And V6O 11 There is a strong transition that involves strong electron correlation, so in V6O 11 There is a small polaron transition phenomenon in it, which can absorb near-infrared light.
[0004] US Patent No. 4372653A discloses a transition material oxide composition (VO, VO2, V2O3, V3O5, V4O7, V5O9, V6O 11 The modulator is composed of a modulator composed of a plurality of optical components (such as a 3D optical modulator, ... 11 The Chinese patent CN107010668B discloses a method for preparing ultrafine Magnéli phase V by high temperature gas phase reduction deposition. n O 2n-1 The invention discloses a device and method for preparing ultrafine Magnéli phase V2O5 by using V2O5 as a vanadium source and sublimating V2O5 first and then cooling it at a high temperature of 1000-1200°C in an atmosphere of CO2 and H2 as reaction gases. n O 2n-1 Powder. The use of H2 atmosphere in a high temperature environment increases the risk of the preparation process. Since its preparation is difficult, the preparation process and equipment are complex and dangerous, there are certain bottlenecks in its development in the field of photocatalysis. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a Magnéli phase V6O 11 A piezoelectric catalyst and a preparation method and application thereof, wherein the catalyst has a good broad-spectrum cyclic degradation effect on organic pollutants under dark conditions and under a full spectrum.
[0006] The present invention is achieved through the following technical solutions:
[0007] The present invention provides a Magnéli phase V6O 11 The method for preparing a piezoelectric catalyst comprises the following steps:
[0008] Step 1: dissolving NH4VO3 in a citric acid solution and stirring evenly to form a precursor solution A; subjecting the precursor solution A to a hydrothermal reaction, separating the obtained product and washing and drying it to obtain powdered NH4(V3O8);
[0009] Step 2: Dissolve VO2 powder and NH4 (V3O8) powder in a mixed solution of isopropanol and H2O, stir evenly to form a precursor solution B, subject the precursor solution B to a hydrothermal reaction, separate the obtained product, wash and dry it, and obtain Magnéli phase V6O 11 Piezoelectric catalyst.
[0010] Preferably, in step 1, the ratio of NH4VO3 to citric acid solution is (11.00-11.15) mmol: (20-30) mL, and the concentration of the citric acid solution is 0.50-0.55 mol / L.
[0011] Preferably, in step 1, the hydrothermal reaction temperature is 100-120° C. and the reaction time is 10 h to 14 h.
[0012] Preferably, in step 2, the preparation method of VO2 powder is: dissolving vanadium acetylacetonate in a mixed solution of isopropanol and water, stirring to form a precursor solution; subjecting the precursor solution to a hydrothermal reaction, separating and precipitating, washing and drying, and obtaining VO2 powder.
[0013] Preferably, in step 2, the mass ratio of VO2 powder and NH4 (V3O8) powder is (2.5-3.5):1.
[0014] Preferably, in step 2, the hydrothermal reaction temperature is 180°C to 200°C, and the time is 0.5h to 3.0h.
[0015] Preferably, in step 2, the volume ratio of isopropanol to H2O is: (11.5-13.5): (11.5-13.5).
[0016] The present invention provides Magnéli phase V6O obtained by the preparation method as described above. 11 Piezoelectric catalyst.
[0017] The present invention provides the Magnéli phase V6O 11 Application of piezoelectric catalysts in degradation of organic pollutants under dark conditions or under light conditions.
[0018] Preferably, the organic pollutant is an antibiotic or an organic matter, the antibiotic is tetracycline or ciprofloxacin; the organic matter is bisphenol A, salicylic acid, coumarin or phenol.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention uses VO2 and NH4 (V3O8) as raw materials, isopropanol and H2O as solvents, and prepares V6O with sponge gourd-like structure at low temperature by hydrothermal method. 11 Nanosheets have simple preparation methods, are easy to operate, and have high safety.
[0021] V6O prepared by the present invention 11 It is a piezoelectric dark catalytic material for energy storage and photothermal energy storage, using V6O 11 A large number of free electrons inside the material and a large number of holes generated by the change of valence of V metal in the material, at the same time, it is disturbed by mechanical stress to form strain. 11The piezoelectric potential is generated inside, thus forming a piezoelectric field. 11 There is a polarization electric field in the crystal, which has piezoelectric properties and can store electrons and holes. In the dark, Magnéli phase V6O 11 The mechanical stress perturbation forms strain, which orients and enhances the internal polarization electric field, and quickly releases the stored electrons and holes in the dark for catalytic reaction. At the same time, the mechanical stress perturbation strain makes the Magnéli phase V6O 11 The piezoelectric catalyst generates piezoelectric charges, and the released stored electron holes and piezoelectric charges degrade organic pollutants. The piezoelectric energy storage effect greatly improves the dark catalytic ability of the material to a level comparable to the photocatalytic ability, so that the material has excellent photocatalytic ability and high-efficiency dark catalytic ability, achieving dark-full-spectrum piezoelectric catalytic ability, good degradation ability for organic pollutants, and good dark cycle stability. In addition, V6O 11 The small polaron transition phenomenon also exists in the degradation process, which increases the temperature of the liquid phase degradation system during the degradation process, has a photothermal effect, accelerates the degradation reaction, and further improves the broad-spectrum degradation ability within the full spectrum. 11 Photothermal energy storage piezoelectric catalysts have good application prospects in water pollution purification in the full spectrum and in the dark. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 is a SEM image of the catalyst prepared in Example 1.
[0024] Figure 2 This is a STEM image of the catalyst prepared in Example 1.
[0025] Figure 3 is the HRTEM image of the catalyst prepared in Example 1.
[0026] Figure 4 It is a phase change diagram of Example 2 of the present invention.
[0027] Figure 5 It is a phase change diagram of Example 3 of the present invention.
[0028] Figure 6 It is a phase change diagram of Example 1 of the present invention.
[0029] Figure 7This is an amplitude variation diagram of Example 2 of the present invention.
[0030] Figure 8 This is an amplitude variation diagram of Example 3 of the present invention.
[0031] Fig. 9 This is an amplitude variation diagram of Example 1 of the present invention.
[0032] Fig.10 It is the degradation curve of 40mg / L tetracycline under visible light for the catalysts prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present invention.
[0033] Fig.11 It is the apparent rate constant of the catalyst prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present invention for 40 mg / L tetracycline under visible light.
[0034] Fig.12 This is a graph showing the TOC removal rate of 40 mg / L tetracycline by the catalyst prepared in Example 1 of the present invention under visible light.
[0035] Fig.13 This is a graph showing the cyclic degradation of 40 mg / L tetracycline by the catalyst prepared in Example 1 of the present invention under visible light.
[0036] Fig.14 This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention under visible light.
[0037] Fig.15 It is the degradation curve of 40 mg / L tetracycline of the catalyst prepared by comparative example 1 and examples 1, 2 and 3 of the present invention under near infrared light.
[0038] Fig.16 It is the apparent rate constant of the catalyst prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present invention for 40 mg / L tetracycline under near infrared light.
[0039] Fig.17 This is a graph showing the TOC removal rate of 40 mg / L tetracycline by the catalyst prepared in Example 1 of the present invention under near-infrared light.
[0040] Fig.18 This is a graph of the cyclic degradation of 40 mg / L tetracycline by the catalyst prepared in Example 1 of the present invention under near-infrared light.
[0041] Fig.19 This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention under near-infrared light.
[0042] Fig. 20 This is an infrared temperature imaging diagram of the catalyst prepared in Example 1 of the present invention degrading 40 mg / L tetracycline for 90 minutes under visible light.
[0043] Fig.21 This is an infrared temperature imaging diagram of the catalyst prepared in Example 1 of the present invention degrading 40 mg / L tetracycline for 90 minutes under near-infrared light.
[0044] Fig. 22 It is a degradation curve diagram of 40 mg / L tetracycline of the catalyst prepared in Example 1 of the present invention under monochromatic light of 740 nm, 850 nm, 940 nm and 1100 nm.
[0045] Fig.23 This is a graph showing the degradation rates of 20 mg / L phenol, 20 mg / L ciprofloxacin, 20 mg / L salicylic acid, 20 mg / L bisphenol A and 20 mg / L coumarin by the catalyst prepared in Example 1 of the present invention under visible light.
[0046] Fig.24 This is a graph showing the degradation rates of 20 mg / L phenol, 20 mg / L ciprofloxacin, 20 mg / L salicylic acid, 20 mg / L bisphenol A and 20 mg / L coumarin by the catalyst prepared in Example 1 of the present invention under near-infrared light.
[0047] Fig.25 This is a graph showing the TOC removal rate of the catalyst prepared in Example 1 of the present invention for 20 mg / L phenol, 20 mg / L ciprofloxacin, 20 mg / L salicylic acid, 20 mg / L bisphenol A and 20 mg / L coumarin under visible light.
[0048] Fig.26 This is a graph showing the TOC removal rate of the catalyst prepared in Example 1 of the present invention for 20 mg / L phenol, 20 mg / L ciprofloxacin, 20 mg / L salicylic acid, 20 mg / L bisphenol A and 20 mg / L coumarin under near-infrared light.
[0049] Fig. 27 The removal curve of 40 mg / L tetracycline in the dark by the catalysts prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present invention.
[0050] Fig.28 It is the apparent rate constant of the catalyst prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present invention for 40 mg / L tetracycline in the dark.
[0051] Fig.29 This is a graph of the cyclic degradation of 40 mg / L tetracycline by the catalyst prepared in Example 1 of the present invention after 16 cycles in the dark and then continued in the dark after 30 minutes of illumination.
[0052] Fig.30This is a graph of TOC removal rate of the catalyst prepared in Example 1 of the present invention after 16 cycles of degradation of 40 mg / L tetracycline in the dark, and then continued in the dark after 30 minutes of illumination.
[0053] Fig.31 This is the absorbance curve of the catalyst prepared in Example 1 of the present invention to 70 mg / L methylene blue in the dark.
[0054] Fig.32 This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention in the dark. DETAILED DESCRIPTION
[0055] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0056] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0057] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0058] The Magnéli phase V6O of the present invention 11 The method for preparing a piezoelectric catalyst comprises the following steps:
[0059] Step 1: Dissolve a certain amount of NH4VO3 in a certain concentration of citric acid solution, stir evenly, and form precursor solution A. Transfer the precursor solution A into a polytetrafluoroethylene-lined autoclave for hydrothermal insulation for a period of time, and centrifuge and wash it after cooling to room temperature. Wash the centrifuged powder several times with anhydrous ethanol and deionized water, centrifuge and vacuum dry overnight to obtain powder NH4(V3O8).
[0060] Step 2: Dissolve VO2 and powdered NH4 (V3O8) in a mixed solution of isopropanol and H2O at a certain mass ratio, stir evenly to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave, and hydrothermally heat for a certain period of time. After the solution is cooled, centrifuge to obtain a precipitate, wash the precipitate several times with anhydrous ethanol and deionized water, and vacuum dry overnight to obtain black-green V6O 11 Piezoelectric catalyst.
[0061] In step 1 of the present invention, the ratio of NH4VO3 to citric acid solution is (11.00-11.15) mmol: (20-30) mL, the concentration of the citric acid solution is 0.50-0.55 mol / L, and the mixture is stirred for 20-30 hours to form a precursor solution A. The precursor solution A is transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 40%-60%. The precursor solution A loaded into the polytetrafluoroethylene-lined autoclave is kept warm at 100-120°C for 10-14 hours, cooled to room temperature, and then centrifuged. The centrifuged powder is washed 4 times with anhydrous ethanol and deionized water, respectively. The washed powder is vacuum dried overnight at 50-70°C to obtain powder NH4(V3O8).
[0062] In step 2 of the present invention, VO2 and NH4 (V3O8) powders are dissolved in a mixed solution of 11.5 mL to 13.5 mL isopropanol and 11.5 mL to 13.5 mL H2O at a mass ratio of (2.5 to 3.5):1, stirred for 25 min to 35 min to form a precursor solution, the precursor solution is transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 40% to 60%, and hydrothermally heated at 180° C. to 200° C. for 0.5 h to 3.0 h, after the solution is cooled, centrifuged to obtain a precipitate, washed with anhydrous ethanol and deionized water respectively, and vacuum dried at 50° C. to 70° C. overnight to obtain a black-green V6O 11 Photothermal energy storage piezoelectric catalyst, its chemical formula is V n O 2n-1 (n=3~9).
[0063] Magnéli phase V6O prepared by the present invention 11 It is a triclinic phase structure, space group: P-1(2). Its stored electron concentration is 498.50μmol·g -1 , is an energy storage catalyst; its d 33 The value is 5.70nm·V -1 , with piezoelectric properties; it has good photothermal properties, and the temperature of the reaction system increases by 18.4℃ / 22.5℃ after 90min of visible light / near-infrared light irradiation.
[0064] Therefore, the Magnéli phase V6O prepared in the present invention 11The photothermal piezoelectric catalyst has the effect of catalytically degrading organic pollutants under full spectrum-dark conditions and has good full spectrum-dark cycle stability. The organic pollutants are antibiotics or organic matter, and the antibiotics are tetracycline or ciprofloxacin. The organic matter is bisphenol A, salicylic acid, coumarin or phenol.
[0065] V6O in dark conditions 11 The stored electron holes and newly generated piezoelectric charges released by strain have a good degradation effect on antibiotics and organic matter. 11 It has excellent dark cycle stability, which improves its practical application potential.
[0066] Comparative Example 1
[0067] Step 1, dissolving 0.276 mmol of vanadyl acetylacetonate in a mixed solution of 22.5 mL of isopropanol and 7.5 mL of water, and stirring for 40 min to form a precursor solution A;
[0068] Step 2, placing the precursor solution A in a hydrothermal reactor, with the filling amount of the precursor solution A in the polytetrafluoroethylene liner being 70%, hydrothermally reacting at 190° C. for 3 h, and centrifuging to obtain a precipitate;
[0069] Step 3, wash the precipitate after centrifugation with deionized water and anhydrous ethanol three times respectively, and then vacuum dry it at 60°C for 12 hours to obtain VO2 powder.
[0070] Example 1
[0071] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0072] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0073] Example 2
[0074] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0075] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and heat it at 190 ° C for 0.5 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0076] Example 3
[0077] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0078] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and heat it at 190 ° C for 1 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0079] Example 4
[0080] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0081] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and heat it at 190 ° C for 1.5 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0082] Example 5
[0083] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0084] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and heat it at 190 ° C for 2 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0085] Example 6
[0086] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0087] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and heat it at 190 ° C for 2.5 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0088] Example 7
[0089] Step 1: 11.00mmol of NH4VO3 was dissolved in 25mL of 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0090] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0091] Example 8
[0092] Step 1: Dissolve 11.15mmol of NH4VO3 in 25mL of 0.53mol / L citric acid solution and stir for 24h to form precursor solution A. Transfer the precursor solution A into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and keep it at 110℃ for 12h. After cooling to room temperature, centrifuge and wash it. Wash the centrifuged powder with anhydrous ethanol and deionized water for 4 times, and vacuum dry it at 60℃ overnight to obtain powder M.
[0093] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0094] Example 9
[0095] Step 1: 11.11mmol of NH4VO3 was dissolved in 20mL of 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0096] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0097] Example 10
[0098] Step 1: 11.11mmol NH4VO3 was dissolved in 30mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0099] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0100] Embodiment 11
[0101] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.50mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0102] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0103] Example 12
[0104] Step 1: Dissolve 11.11mmol of NH4VO3 in 25mL of 0.55mol / L citric acid solution and stir for 24h to form precursor solution A. Transfer the precursor solution A into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and keep it at 110°C for 12h. After cooling to room temperature, centrifuge and wash it. Wash the centrifuged powder with anhydrous ethanol and deionized water for 4 times, and vacuum dry it at 60°C overnight to obtain powder M.
[0105] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0106] Example 13
[0107] Step 1: Dissolve 11.11mmol NH4VO3 in 25mL 0.53mol / L citric acid solution and stir for 20h to form precursor solution A. Transfer the precursor solution A into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and keep it at 110℃ for 12h. After cooling to room temperature, centrifuge and wash it. Wash the centrifuged powder with anhydrous ethanol and deionized water for 4 times, and vacuum dry it at 60℃ overnight to obtain powder M.
[0108] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0109] Embodiment 14
[0110] Step 1: Dissolve 11.11mmol of NH4VO3 in 25mL of 0.53mol / L citric acid solution and stir for 30h to form precursor solution A. Transfer the precursor solution A into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and keep it at 110°C for 12h. After cooling to room temperature, centrifuge and wash it. Wash the centrifuged powder with anhydrous ethanol and deionized water for 4 times, and vacuum dry it at 60°C overnight to obtain powder M.
[0111] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0112] Embodiment 15
[0113] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 40%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0114] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0115] Example 16
[0116] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 60%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0117] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0118] Embodiment 17
[0119] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 100°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0120] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0121] Embodiment 18
[0122] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 120°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0123] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0124] Embodiment 19
[0125] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 10h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0126] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0127] Embodiment 20
[0128] Step 1: 11.11mmol of NH4VO3 was dissolved in 25mL of 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 14h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0129] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0130] Embodiment 21
[0131] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 50°C overnight to obtain powder M.
[0132] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0133] Embodiment 22
[0134] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 70°C overnight to obtain powder M.
[0135] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0136] Embodiment 23
[0137] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0138] Step 2: VO2 and powder M were dissolved in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 2.5:1, stirred for 30 min to form precursor solution B, and the precursor solution B was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally insulated at 190 ° C for 3 h. After the solution was cooled, it was centrifuged to obtain a precipitate and washed. The precipitate was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0139] Embodiment 24
[0140] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0141] Step 2: VO2 and powder M were dissolved in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3.5:1, stirred for 30 min to form precursor solution B, and the precursor solution B was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally insulated at 190 ° C for 3 h. After the solution was cooled, it was centrifuged to obtain a precipitate and washed. The precipitate was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0142] Embodiment 25
[0143] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0144] Step 2: VO2 and powder M were dissolved in a mixed solution of 11.5 mL isopropanol and 11.5 mL H2O at a mass ratio of 3:1, stirred for 30 min to form precursor solution B, and the precursor solution B was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally insulated at 190 ° C for 3 h. After the solution was cooled, it was centrifuged to obtain a precipitate and washed. The precipitate was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0145] Embodiment 26
[0146] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0147] Step 2: Dissolve VO2 and powder M in a mixed solution of 13.5 mL isopropanol and 13.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0148] Embodiment 27
[0149] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0150] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 25 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0151] Embodiment 28
[0152] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0153] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 35 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0154] Embodiment 29
[0155] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0156] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 40%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0157] Embodiment 30
[0158] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0159] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 60%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0160] Embodiment 31
[0161] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0162] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 180°C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 60°C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0163] Embodiment 32
[0164] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0165] Step 2: VO2 and powder M were dissolved in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stirred for 30 min to form precursor solution B, and the precursor solution B was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally insulated at 200 ° C for 3 h. After the solution was cooled, it was centrifuged to obtain a precipitate and washed. The precipitate was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0166] Embodiment 33
[0167] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0168] Step 2: Dissolve VO2 and powder M in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stir for 30 min to form precursor solution B, transfer precursor solution B into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally heat at 190 ° C for 3 h. After the solution is cooled, centrifuge to obtain a precipitate and wash it. Wash the precipitate with anhydrous ethanol and deionized water 4 times, and vacuum dry it at 50 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0169] Embodiment 34
[0170] Step 1: 11.11mmol NH4VO3 was dissolved in 25mL 0.53mol / L citric acid solution and stirred for 24h to form precursor solution A. Precursor solution A was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and kept at 110°C for 12h. After cooling to room temperature, it was centrifuged and washed. The centrifuged powder was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 60°C overnight to obtain powder M.
[0171] Step 2: VO2 and powder M were dissolved in a mixed solution of 12.5 mL isopropanol and 12.5 mL H2O at a mass ratio of 3:1, stirred for 30 min to form precursor solution B, and the precursor solution B was transferred into a polytetrafluoroethylene-lined autoclave with a filling amount of 50%, and hydrothermally insulated at 190 ° C for 3 h. After the solution was cooled, it was centrifuged to obtain a precipitate and washed. The precipitate was washed 4 times with anhydrous ethanol and deionized water, and vacuum dried at 70 ° C overnight to obtain black-green V6O 11 Piezoelectric catalysts for photothermal energy storage.
[0172] The above conclusions and mechanisms are explained in detail below.
[0173] Figure 1 is a SEM image of the catalyst prepared in Example 1. 11 It is an irregular flake structure formed by stacking flakes of different sizes. Figure 2 This is a STEM image of the catalyst prepared in Example 1. 11 From the STEM image, we can see that V6O 11 When the nanosheets are magnified, they appear to have a loofah-like structure, with a large number of pores of about 2 nm in size. Figure 3 This is the HRTEM image of the catalyst prepared in Example 1. 11 The lattice fringe spacings in the HRTEM image are 0.331 nm, 0.306 nm, and 0.257 nm, corresponding to the (-120), (-1-17), and (-205) crystal planes, further indicating the formation of flake V6O 11 .
[0174] Figure 4 , Figure 5 and Figure 6 They are phase change diagrams of Example 2, Example 3 and Example 1. After applying a deflection voltage of 10V, the phase angle flips by about 180°, proving that the dipole is easily transformed by an external electric field.
[0175] Figure 7 , Figure 8 and Fig. 9 The amplitude change diagrams of Example 2, Example 3 and Example 1 are shown respectively. Under the action of the electric field, the samples prepared in the three examples all showed a typical "butterfly-shaped curve", producing a strain-electric field hysteresis phenomenon, proving that V6O 11 The piezoelectric response is obvious. The piezoelectric "butterfly curve" is used to calculate the d of Example 2, Example 3 and Example 1. 33 The values are 2.25, 2.55, and 5.70 nm·V respectively. -1 , proves that V6O 11It has better piezoelectric properties. The larger piezoelectric polarization characteristics can induce the energy storage catalyst to store charge and generate piezoelectric charge under mechanical stress, thereby improving the catalytic activity under dark conditions. Therefore, when mechanical stress perturbs the strain, V6O 11 Photothermal energy storage piezoelectric catalysts store and generate piezoelectric charges, and the released stored charges and the newly generated piezoelectric charges undergo redox reactions, thereby converting V6O 11 It has strong dark catalytic ability.
[0176] Fig.10 and Fig.11 The degradation curves and apparent rate constants of the catalysts prepared in Comparative Example 1 and Examples 2, 3, and 1 for 40 mg / L tetracycline under visible light are shown. After 90 minutes of reaction under direct visible light irradiation, the degradation rates of Comparative Example 1, Example 2, Example 3, and Example 1 for 40 mg / L TC are 82.00%, 71.38%, 73.28%, and 92.02%, respectively, and the apparent rate constants of each sample are 0.02376 min -1 、0.01780min -1 、0.01894min -1 、0.03781min -1 . Fig.12 and Fig.13 The TOC removal rate and cyclic degradation diagram of the catalyst prepared in Example 1 of the present invention for 40 mg / L tetracycline under visible light. 11 After 90 minutes of direct visible light irradiation, the TOC removal rate of 40 mg / L TC reached 79.74%, indicating that it has good mineralization ability. 11 After four cycles of degradation under direct visible light irradiation, the efficiency remained at 89.09%, and the degradation activity decreased by only 4.57% compared with the first degradation, indicating that it has good cyclic stability under direct visible light irradiation.
[0177] Fig.14 This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention under visible light. 11 Under direct visible light irradiation, the photocatalytic performance of BQ, Na2C2O4, TBA (t-BuOH) and CuSO4 decreased by 22.44%, 14.29%, 6.90% and 6.03% respectively. This indicates that during the degradation reaction under direct visible light irradiation, ·O2 - is the main active species, followed by h + , OH and e - .
[0178] Fig.15 and Fig.16The degradation curves and apparent rate constants of the catalysts prepared in Comparative Example 1 and Examples 2, 3, and 1 of the present invention for 40 mg / L tetracycline under near-infrared light. After 90 minutes of reaction under direct near-infrared light irradiation, the degradation rates of Comparative Example 1, Example 2, Example 3, and Example 1 for 40 mg / L TC are 83.04%, 61.54%, 60.09%, and 92.49%, respectively. The apparent rate constants of the samples are 0.02575 min -1 (Comparative Example 1), 0.01355min -1 (Example 2), 0.01235min -1 (Example 3) and 0.03556min -1 (Example 1). Fig.17 and Fig.18 Figure 1 is a TOC removal rate diagram and cyclic degradation diagram of the catalyst prepared in Example 1 of the present invention for 40 mg / L tetracycline under near infrared light. After 90 minutes of direct near infrared light irradiation, V6O 11 The TOC removal rate of 40 mg / L TC reached 80.13%, indicating that it also has excellent mineralization effect under near-infrared light. 11 Under the condition of direct irradiation of near-infrared light, four cycles of degradation were carried out, and the degradation rates were 92.71%, 92.50%, 92.25% and 89.07% respectively. After four cycles, the degradation activity only decreased by 3.64%, and the reason for the decrease in activity may be due to the small loss of powder. It shows that it has excellent cyclic stability under direct irradiation of near-infrared light.
[0179] Fig.19 This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention under near-infrared light. Under near-infrared light direct irradiation, after adding BQ, Na2C2O4, TBA and CuSO4, the degradation ability of the photocatalyst decreased from 92.49% to 83.69%, 39.29%, 75.69% and 83.02% respectively. + are the main active substances in the degradation process, while ·OH, ·O2 - and e - It plays a minor role in the degradation process.
[0180] Fig. 20 and Fig.21 This is an infrared temperature image of the catalyst prepared in Example 1 of the present invention degrading 40 mg / L tetracycline for 90 minutes under visible light and near infrared light. The corresponding temperature changes during the degradation process were observed using an infrared thermal imager to verify that V6O 11 Photothermal effect in liquid phase. After 90 min of direct irradiation with visible light / near infrared light, V6O 11The solution temperature of V6O increased by about 32℃ / 38.2℃ respectively. 11 It not only has good photothermal performance under visible light, but also has excellent photothermal effect under near-infrared light.
[0181] Fig. 22 The degradation curve of the catalyst prepared in Example 1 of the present invention for 40 mg / L tetracycline under monochromatic light of 740 nm, 850 nm, 940 nm and 1100 nm was shown in Figure 2. The degradation experiment was carried out under monochromatic light irradiation conditions, further proving that V6O 11 It has a degradation effect on TC in the full spectrum. After 90 minutes of direct irradiation with 740nm, 850nm, 940nm and 1100nm monochromatic light, the degradation rates of 40mg / L TC are 58.95%, 63.62%, 64.11% and 61.21% respectively. This shows that V6O 11 It has enhanced photocatalytic degradation activity for TC under the full spectrum and has practical application prospects.
[0182] Fig.23 and Fig.24 This is a graph showing the degradation rates of 20 mg / L phenol, 20 mg / L ciprofloxacin, 20 mg / L salicylic acid, 20 mg / L bisphenol A and 20 mg / L coumarin by the catalyst prepared in Example 1 of the present invention under visible light and near-infrared light. Fig.25 and Fig.26 The figure is the removal rate of 20mg / L phenol, 20mg / L ciprofloxacin, 20mg / L salicylic acid, 20mg / L bisphenol A and 20mg / L TOC by the catalyst prepared in Example 1 of the present invention under visible light and near infrared light. Under direct visible light irradiation for 90min, the degradation rates of 20mg / L phenol, CIP, BHA, BPA and coumarin are 68.29%, 92.87%, 63.89%, 56.89% and 70.08% respectively; under direct near infrared light irradiation for 90min, the maximum degradation rates of phenol, CIP, BHA, BPA and coumarin are 61.43%, 82.39%, 61.63%, 48.92% and 69.98% respectively. It shows that V6O 11 It has excellent broad-spectrum degradation effect in the whole spectrum. After 90 minutes of direct irradiation with visible light and near-infrared light, V6O 11 The TOC removal rates of phenol, CIP, BHA, BPA and coumarin were 50.52% / 48.90%, 76.84% / 66.33%, 51.87% / 53.96%, 45.82% / 36.57% and 63.69% / 54.44%, respectively, indicating that V6O 11 It has good broad-spectrum mineralization ability over the full spectrum.
[0183] Fig. 27 and Fig.28 The removal curves and apparent rate constants of 40 mg / L tetracycline under dark conditions for the catalysts prepared by comparative example 1 and examples 2, 3, and 1 of the present invention. After 90 minutes of dark reaction, the dark catalytic activity of example 1 (87.82%) is significantly higher than that of example 2 (52.06%), example 3 (56.46%), and comparative example 1 (64.28%). The degradation rates of comparative example 1, example 2, example 3, and example 1 are 0.01477 min -1 、0.00954min -1 、0.01105min -1 and 0.02559min -1 . Fig.29 and Fig.30 The cyclic degradation graph and TOC removal rate graph of the catalyst prepared in Example 1 of the present invention after 16 cycles in the dark and then continued in the dark after 30 minutes of illumination. 11 The dark catalytic degradation activity of 40 mg / L TC can be maintained for 16 reaction cycles. With the extension of reaction time, the degradation rate gradually decreases, which is attributed to the consumption of stored electrons and holes and the loss of some powders. In addition, during the 1st, 4th, 7th, 10th, 13th and 16th cycle reactions, the degradation rate of V6O 11 The TOC removal rates for 40 mg / L TC were 78.33%, 72.32%, 68.83%, 63.98%, 60.49% and 53.71%, respectively, indicating that V6O 11 The mineralization capacity of V6O was also high in the dark. 11 The long-term dark catalytic activity and high mineralization capacity of V6O can be restored, proving that 11 It has good stability and repairability.
[0184] Fig.31 The absorbance curve of the catalyst prepared in Example 1 of the present invention to 70 mg / L methylene blue in the dark. The electron concentration stored in the sample was estimated by the titration experiment of methylene blue, and the V6O 11 The electron concentration stored in is 498.50 μmol·g -1 . Fig.32This is a capture diagram of active species of the catalyst prepared in Example 1 of the present invention in the dark. After introducing BQ, Na2C2O4, TBA and CuSO4 into the degradation reaction system under dark conditions, the degradation rate of 40mg / L TC decreased from 87.82% to 77.58%, 52.89%, 43.99% and 72.53% respectively. Subsequently, BQ and TBA were introduced into the system at the same time, and the degradation rate decreased by 12.10%, which proved that O2 - 、h + , OH and e - They all play a role to a certain extent during the dark reaction.
[0185] The present invention utilizes V6O 11 A large number of free electrons inside the material and a large number of holes generated by the change of valence of V metal in the material, at the same time, it is disturbed by mechanical stress to form strain. 11 A piezoelectric potential is generated inside the material, which in turn forms a piezoelectric field, greatly improving the dark catalytic ability of the material to a level comparable to its photocatalytic ability. It has good degradation capabilities for the antibiotic tetracycline, ciprofloxacin, and the organic substances bisphenol A, salicylic acid, phenol, and coumarin. A material with excellent photocatalytic ability and high-efficiency dark catalytic ability has been successfully prepared.
[0186] The above is only one embodiment of the present invention, not all or the only embodiment. Any equivalent changes made to the technical solution of the present invention by ordinary technicians in this field after reading the specification of the present invention are covered by the claims of the present invention.
Claims
1. A Magnéli phase V6O 11 A method for preparing a piezoelectric catalyst, characterized in that: The following steps are involved: Step 1: dissolving NH4VO3 in a citric acid solution and stirring evenly to form a precursor solution A; subjecting the precursor solution A to a hydrothermal reaction, separating the obtained product and washing and drying it to obtain powdered NH4(V3O8); Step 2: Dissolve VO2 powder and NH4 (V3O8) powder in a mixed solution of isopropanol and H2O, stir evenly to form a precursor solution B, subject the precursor solution B to a hydrothermal reaction, separate the obtained product, wash and dry it, and obtain Magnéli phase V6O 11 Piezoelectric catalyst.
2. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 1, the ratio of NH4VO3 to citric acid solution is (11.00-11.15) mmol: (20-30) mL, and the concentration of citric acid solution is 0.50-0.55 mol / L.
3. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 1, the hydrothermal reaction temperature is 100-120° C. and the reaction time is 10 h-14 h.
4. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 2, the preparation method of VO2 powder is: dissolving vanadium acetylacetonate in a mixed solution of isopropanol and water, stirring to form a precursor solution; subjecting the precursor solution to a hydrothermal reaction, separating and precipitating, washing and drying, and obtaining VO2 powder.
5. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 2, the mass ratio of VO2 powder and NH4 (V3O8) powder is (2.5-3.5):
1.
6. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 2, the hydrothermal reaction temperature is 180° C. to 200° C., and the reaction time is 0.5 h to 3.0 h.
7. Magneli phase V6O according to claim 1 11 A method for preparing a piezoelectric catalyst, characterized in that: In step 2, the volume ratio of isopropanol and H2O is: (11.5-13.5): (11.5-13.5).
8. Magneli phase V6O obtained by the preparation method according to any one of claims 1 to 7 11 Piezoelectric catalyst.
9. The Magnéli phase V6O according to claim 8 11 Application of piezoelectric catalysts in degradation of organic pollutants under dark conditions or under light conditions.
10. The use according to claim 9, characterized in that: The organic pollutant is an antibiotic or an organic matter, the antibiotic is tetracycline or ciprofloxacin; the organic matter is bisphenol A, salicylic acid, coumarin or phenol.
Citation Information
Patent Citations
Equipment and method for preparing ultrafine magnéli phase vno2n-1 powder by high-temperature vapor phase reduction deposition
CN107010668B
Polarizing beam splitting phase transition optical modulator
US4372653A
Equipment and method for preparing superfine Magneli-phase VnO2n-1 powder through high-temperature vapor reduction deposition
CN107010668A
V2O3 / VO2 composite electrocatalyst and preparation method thereof
CN109201038A
Method for preparing quadrangular tubular nanocrystals NH4V3O8
CN110217820A