Preparation method and application of ReS2 two-dimensional superlattice structure

By growing ReS2 nanosheets with a single layer of carbon intercalated ReS2 on carbon-based materials, forming a ReS2 two-dimensional superlattice structure, the problem of poor cycling stability of potassium and sodium ion battery anode materials under high current density is solved, and high Performance of electrochemical storage and long-term cycle stability, suitable for negative electrode materials for potassium and sodium ion batteries.

CN118929763AActive Publication Date: 2024-11-12HEFEI UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411007184.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The negative electrode materials of potassium ion batteries and sodium ion batteries have poor cycling stability under high current density and are easily damaged, resulting in low long-term cycle stability and reversible specific capacity of batteries. The negative electrode materials of traditional lithium ion batteries are not suitable and are difficult to replace.

Method used

A preparation method of ReS2 two-dimensional superlattice structure is adopted. By growing ReS2 nanosheets with a single layer of carbon intercalated layer on carbon-based materials, the layer spacing and electron conductivity are adjusted, and a stable conductive network is formed to improve solid-solid reaction. Active, suitable for negative electrode materials for potassium or sodium ion batteries.

Benefits of technology

It realizes high electrochemical storage performance of ReS2 two-dimensional superlattice structure, exhibits excellent rate performance and long-term cycle life, has excellent potassium or sodium storage performance, and is simple in process and low in cost, suitable for quantitative production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004963305130000011
    Figure HDA0004963305130000011
  • Figure HDA0004963305130000012
    Figure HDA0004963305130000012
  • Figure HDA0004963305130000021
    Figure HDA0004963305130000021
Patent Text Reader

Abstract

The invention provides a preparation method and application of a ReS2 two-dimensional superlattice structure, single-layer carbon is inserted between two adjacent ReS2 single-molecule nano layers, and the ReS2 two-dimensional superlattice structure has multiple effects: the interlayer spacing of ReS2 can be widened, and alkali metal ions can be conveniently and rapidly inserted / removed; the surface and internal electron conductivity of ReS2 can be improved, so that electron transmission is fully accelerated; in addition, ReS2 is confined between two single-layer carbon structures, so that the solid-solid reaction activity in the charge-discharge process is improved. The unique nano-structure can also form a conductive network with a carbon-based material to form a firm frame, and has excellent nano-structure stability. The obtained product is unique in structure, regular in morphology, uniform in component, free of impurity phase and excellent in electrochemical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical energy storage, and specifically relates to a method for preparing a ReS2 two-dimensional superlattice structure and its application in potassium ion batteries or sodium ion batteries. Background Art

[0002] Lithium-ion batteries have been widely studied and applied to electronic products of all sizes. Today, the demand for lithium resources has increased dramatically, which will directly lead to the problem of lithium resource shortage. The abundance of potassium and sodium resources in the earth's crust is about 1,000 times that of lithium. Potassium ions and sodium ions have many physical and chemical properties similar to lithium ions. The operating principles of potassium ion batteries and sodium ion batteries are also similar to those of lithium ion batteries. Based on these advantages and similarities, potassium ion batteries and sodium ion batteries are ideal substitutes for lithium ion batteries. However, potassium ions and sodium ions ( and ) has a much larger ionic radius than lithium ions This means that when using the negative electrode of a conventional lithium-ion battery, large-sized ion insertion / extraction leads to the destruction of the negative electrode material structure, slow diffusion kinetics, low structural stability and other problems. Therefore, it is particularly important to develop a stable and adaptable structure to ensure the long-term cycle stability and high reversible specific capacity of the battery.

[0003] Transition metal dichalcogenides (TMDs) have unique physical and chemical properties and are considered to be one of the most promising negative electrode materials for alkali ion batteries. Among them, rhenium disulfide (ReS2) nanosheets have a large interlayer spacing (0.61nm) and a high theoretical specific capacity (428mAh g -1 ), has been widely studied in sodium-ion batteries, but its cycling stability at higher current density and its application in potassium-ion batteries have rarely been reported. In view of the low intrinsic conductivity of ReS2 nanosheet layered materials and the structural collapse caused by volume change during charging and discharging, modifying the ReS2 nanosheet structure is a common and effective strategy. Ions, atoms, molecules and polymers can be inserted into the van der Waals gaps between adjacent layers of layered two-dimensional materials without destroying the covalent bonds within the layers. By adjusting the structure, composition and size of the inserted guest material and host material, a series of layered insertion materials can be prepared, which have highly adjustable chemical and physical properties compared to the original materials. Due to the two-dimensional layered characteristics of ReS2, the synthesis of stable layer space widening, internal conductivity enhancement and ReS2 advanced composite materials with two-dimensional confined space for rapid potassium or sodium ion extraction has important research value and practical application significance. Summary of the invention

[0004] The present invention solves the problems of high cost, long cycle, and difficulty in mass production in the production of high-performance ultra-stable potassium ion batteries or sodium ion batteries. It provides a ReS2 two-dimensional superlattice structure with low cost, simple preparation process, and suitable for mass production, as well as its application in potassium ion batteries or sodium ion batteries. The material of the present invention has outstanding electrochemical storage performance.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for preparing a ReS2 two-dimensional superlattice structure comprises the following steps:

[0007] Step 1, weigh 2-6 mmol CH4N2S or C2H5NS and add it to 3-10 mL of deionized water, stir for 1-20 minutes to obtain solution A;

[0008] Step 2, add 20-400 mg of carbon-based material to 15-30 mL of deionized water, ultrasonicate for 0.1-5 hours, stir for 0.1-2 hours, continue to add 0.5-1.5 mmol of NH4ReO4 and 2-6 mmol of NH3OHCl, stir for 1-40 minutes, and obtain solution B;

[0009] Step 3, adding 1-6 mL of an amino compound and 0.5-8 g of a reducing sugar to the solution B in sequence, stirring for 1-20 minutes, to obtain a solution C;

[0010] Step 4, quickly transferring the solution C into the solution A, sealing and stirring for 10-40 minutes to obtain a mixed solution; transferring the mixed solution into a reaction kettle and reacting at 160-220° C. for 12-24 hours to obtain an initial product;

[0011] Step 5, centrifugally washing the initial product and then drying it in a vacuum drying oven to obtain an intermediate product;

[0012] Step 6: Place the intermediate product in a tubular furnace, then heat it to 500-900°C under a vacuum environment, keep it warm for 1-3 hours, and finally cool it to room temperature to obtain the target product ReS2 two-dimensional superlattice structure, that is, a single-layer carbon-intercalated ReS2 nanosheet grown on a carbon-based material.

[0013] Preferably, the carbon-based material is one of reduced graphene oxide (rGO), carbon nanotubes (CNT), carbon cloth (CC), carbon nanowires (CNW) and carbon spheres (HCS).

[0014] Preferably, the amino compound is ethylenediamine.

[0015] Preferably, the reducing sugar is glucose.

[0016] Preferably, the cleaning in step 5 is performed by sequentially cleaning with deionized water and anhydrous ethanol.

[0017] The ReS2 two-dimensional superlattice structure prepared by the present invention can be used as a negative electrode material in potassium ion batteries or sodium ion batteries.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0019] 1. The present invention provides a method for preparing a ReS2 two-dimensional superlattice structure. The obtained product has a unique structure, regular morphology, uniform composition, no impurity phase, and excellent electrochemical properties.

[0020] 2. A ReS2 two-dimensional superlattice structure prepared by the present invention inserts a single layer of carbon between two adjacent ReS2 monomolecular nanolayers, which has multiple effects: not only can the interlayer spacing of ReS2 be widened to facilitate the rapid insertion / extraction of potassium or sodium ions; but also the surface and internal electronic conductivity of ReS2 can be improved to fully accelerate the transmission of electrons; in addition, ReS2 is confined between two monolayers of carbon, which improves the solid-solid reaction activity. Such a unique nanostructure can also form a conductive network with carbon-based materials to form a solid framework with excellent nanostructure stability.

[0021] 3. The ReS2 superlattice structure prepared by the present invention exhibits excellent rate performance and excellent long-term cycle life at high current density, and has excellent potassium or sodium storage performance.

[0022] 4. The present invention explores an economical and simple method of combined modulation of layered ReS2 through interlayer regulation and nano-level engineering to obtain advanced electrodes for high-performance rechargeable batteries, providing an effective synthesis scheme for the practical application of advanced negative electrode materials for potassium ion batteries and sodium ion batteries.

[0023] 5. The preparation process of the present invention is simple, the preparation cost is low, and it is easy to synthesize in large quantities and promote. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 These are SEM images of samples prepared in Examples 1 to 4 of the present invention, where a, b, c, and d correspond to sample 1 (ReS2@C), sample 2 (rGO@ReS2@C), sample 3 (CNT@ReS2@C), and sample 4 (CC@ReS2@C), respectively.

[0025] Figure 2TEM images of the samples prepared in Examples 1 to 4 of the present invention, where a, b, c and d correspond to sample 1 (ReS2@C), sample 2 (rGO@ReS2@C), sample 3 (CNT@ReS2@C) and sample 4 (CC@ReS2@C), respectively.

[0026] Figure 3 This is the XPS graph of ReS2@C prepared in Example 1 of the present invention, where a, b, c, and d correspond to Re 4f, S2p, C 1s, and N1s, respectively.

[0027] Figure 4 This is the XRD spectrum of the sample prepared in the embodiment of the present invention.

[0028] Figure 5 This is the Raman spectrum of the sample prepared in the embodiment of the present invention.

[0029] Figure 6 The variable rate performance curve of the potassium ion battery assembled from the samples of the present invention.

[0030] Figure 7 The potassium ion battery assembled by the sample of the present invention is –1 The long cycle performance diagram below.

[0031] Figure 8 The potassium ion battery assembled by the sample of the present invention has a high current density of 2A. –1 The long cycle performance diagram below.

[0032] Fig. 9 The sodium ion battery assembled by the sample of the present invention has a high current density of 5Ag –1 The long cycle performance diagram below. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is described in detail below in conjunction with the embodiments. The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0034] In the following process steps of the embodiments, unless otherwise specified, all are carried out at room temperature.

[0035] Example 1

[0036] In this embodiment, ReS2@C is prepared according to the following steps:

[0037] Step 1: Weigh 3 mmol CH4N2S and add it to 5 mL of deionized water. Stir for 10 minutes to obtain solution A.

[0038] Step 2: Weigh 1 mmol of NH4ReO4 and 5.7 mmol of NH3OHCl in 21 mL of deionized water and stir for 30 minutes to obtain solution B.

[0039] Step 3: Add 4 mL of C2H8N2 and 1 g of glucose to the above solution B in sequence, and continue stirring for 15 minutes to obtain solution C.

[0040] Step 4: Rapidly transfer the above solution C to solution A, continue to seal the beaker with sealing glue and stir for 30 minutes to obtain a mixed solution; transfer the mixed solution to a 50 mL reactor and react at 200° C. for 24 hours to obtain an initial product.

[0041] Step 5: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 60° C. and dried for 12 hours to obtain an intermediate product.

[0042] Step 6: Place the intermediate product in a tubular furnace, then heat it to 600°C at a heating rate of 5°C / min under a vacuum environment, keep it warm for 2 hours, and finally cool it naturally to room temperature to obtain the target product ReS2@C, which is recorded as sample 1.

[0043] Example 2

[0044] In this example, rGO@ReS2@C was prepared according to the following steps:

[0045] Step 1: Weigh 3 mmol CH4N2S and add it to 5 mL of deionized water. Stir for 10 minutes to obtain solution A.

[0046] Step 2: Take 4.5 mL of 4.5 mg mL –1 The GO solution was ultrasonicated in 16.5 mL of deionized water for 2 h, stirred for 1 h, and then 1 mmol of NH4ReO4 and 5.7 mmol of NH3OHCl were added and stirred for 20 min to obtain solution B.

[0047] Step 3: Add 4 mL of C2H8N2 and 1 g of glucose to the above solution B in sequence, and stir for 15 minutes to obtain solution C.

[0048] Step 4: Rapidly transfer the above solution C to solution A, continue to seal the beaker with sealing glue and stir for 30 minutes to obtain a mixed solution; transfer the mixed solution to a 50 mL reactor and react at 200° C. for 24 hours to obtain an initial product.

[0049] Step 5: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 60° C. and dried for 12 hours to obtain an intermediate product.

[0050] Step 6: Place the intermediate product in a tubular furnace, then heat it to 600°C at a heating rate of 5°C / min under a vacuum environment, keep it warm for 2 hours, and finally cool it naturally to room temperature to obtain the target product rGO@ReS2@C, which is recorded as sample 2.

[0051] Example 3

[0052] In this example, CNT@ReS2@C was prepared according to the following steps:

[0053] Step 1: Weigh 3 mmol CH4N2S and add it to 5 mL of deionized water. Stir for 10 minutes to obtain solution A.

[0054] Step 2: Take 50 mg of CNT and place it in 21 mL of deionized water for 2 hours under ultrasonication, then stir for 1 hour, and then continue to add 1 mmol of NH4ReO4 and 5.7 mmol of NH3OHCl and stir for 20 minutes to obtain solution B.

[0055] Step 3: Add 4 mL of C2H8N2 and 1 g of glucose to the above solution B in sequence, and stir for 15 minutes to obtain solution C.

[0056] Step 4: Rapidly transfer the above solution C to solution A, continue to seal the beaker with sealing glue and stir for 30 minutes to obtain a mixed solution; transfer the mixed solution to a 50 mL reactor and react at 200° C. for 24 hours to obtain an initial product.

[0057] Step 5: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 60° C. and dried for 12 hours to obtain an intermediate product.

[0058] Step 6: Place the intermediate product in a tubular furnace, then heat it to 600°C at a heating rate of 5°C / min under a vacuum environment, keep it warm for 2 hours, and finally cool it naturally to room temperature to obtain the target product CNT@ReS2@C, recorded as sample 3.

[0059] Example 4

[0060] In this example, CC@ReS2@C was prepared according to the following steps:

[0061] Step 1: Weigh 3 mmol CH4N2S and add it to 5 mL of deionized water. Stir for 10 minutes to obtain solution A.

[0062] Step 2: Take CC (about 300 mg) with a length and width of 5 cm and place it in 21 mL of deionized water for 2 hours, stir it for 1 hour, and continue to add 1 mmol of NH4ReO4 and 5.7 mmol of NH3OHCl and stir it for 20 minutes to obtain solution B.

[0063] Step 3: Add 4 mL of C2H8N2 and 1 g of glucose to the above solution B in sequence, and stir for 15 minutes to obtain solution C.

[0064] Step 4: Rapidly transfer the above solution C to solution A, continue to seal the beaker with sealing glue and stir for 30 minutes to obtain a mixed solution; transfer the mixed solution to a 50 mL reactor and react at 200° C. for 24 hours to obtain an initial product.

[0065] Step 5: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 60° C. and dried for 12 hours to obtain an intermediate product.

[0066] Step 6: Place the intermediate product in a tube furnace, then heat it to 600°C at a heating rate of 5°C / min under a vacuum environment, keep it warm for 2 hours, and finally cool it naturally to room temperature to obtain the target product CC@ReS2@C, which is recorded as sample 4.

[0067] Figure 1 The SEM images of the samples obtained in each embodiment, a, b, c and d in the figure correspond to sample 1 (ReS2@C), sample 2 (rGO@ReS2@C), sample 3 (CNT@ReS2@C) and sample 4 (CC@ReS2@C). The ReS2 nanosheets prepared in sample 1 (ReS2@C) are accumulated into large nanospheres through the carbon wrapping during the hydrothermal process; the ReS2 nanosheets and monolayer carbon in sample 2 (rGO@ReS2@C) are alternately stacked and curled and evenly distributed on rGO; the ReS2 nanosheets in sample 3 (CNT@ReS2@C) are stacked and evenly distributed on CNT. In sample 4 (CC@ReS2@C), ReS2 grows on the surface of carbon cloth (CC).

[0068] Figure 2TEM images of the samples obtained in the above examples, where a, b, c and d correspond to sample 1 (ReS2@C), sample 2 (rGO@ReS2@C), sample 3 (CNT@ReS2@C) and sample 4 (CC@ReS2@C), respectively. Sample 1 (ReS2@C) shows that the ReS2 nanosheets are peeled off into a few layers, and the ReS2 is completely coated by amorphous carbon, and the amorphous carbon is inserted inside to form a two-dimensional superlattice interlayer extension structure. The measured interlayer spacing is 0.90nm. In sample 2 (rGO@ReS2@C), the ReS2 orderly distributed on the rGO is stacked by multi-layer nanosheets with good crystallinity. Two adjacent ReS2 monolayers are intercalated with an amorphous carbon monolayer, forming a two-dimensional superlattice interlayer extension structure in which ReS2 and monolayer carbon overlap each other. The (001) crystal plane of ReS2 is measured to be extended to 0.98nm. Similarly, the nanosheets uniformly distributed on CNT and CC in sample 3 (CNT@ReS2@C) and sample 4 (CC@ReS2@C) are stacked by ReS2 with better crystallinity.

[0069] Figure 3 a, b, c, and d in the figure are the high-resolution Re 4f, S2p, C 1s, and N 1s XPS spectra of sample 1 (ReS2@C), respectively. Figure 3 The peaks at 44.33 and 41.93 eV in a correspond to Re 4f5 / 2 and Re 4f7 / 2, indicating that Re is in the +4 valence state, while the peaks at 45.48 and 42.28 eV belong to the Re–O bonds caused by slight surface oxidation. Figure 3 b is the high-resolution spectrum of S2p. The peaks at 163.28 and 162.23 eV correspond to S2p1 / 2 and S2p3 / 2, corresponding to S 2– Valence. Figure 3 c is the high-resolution spectrum of C1s, and the peaks appearing at 288.23, 285.63, and 284.63 eV correspond to C=O, CN, and CC chemical bonds, respectively. Figure 3 d is the high-resolution spectrum of N1s, which can be divided into two different peaks of nitrogen species, pyrrolic–N at 401.03 eV and pyridinic–N at 398.68 eV. The electrochemically active pyridinic–N and pyrrolic–N can provide abundant external defects and active sites. The doping of carbon with N element further improves the electronic conductivity of carbon.

[0070] Figure 4The XRD diagram of the sample obtained in the above embodiment. Compared with the diffraction peak of ReS2 (JCPDS 52-0818), the most significant (001) diffraction peak is located at 14.59°, corresponding to a ReS2 (001) crystal plane interlayer spacing of 0.61nm. The ReS2 (001) diffraction peak of sample 1 (ReS2@C), sample 2 (rGO@ReS2@C) and sample 3 (CNT@ReS2@C) moves from 14.59° to around 8.99°. The calculation by the Scherrer equation 2dsinθ=nλ shows that the (001) crystal plane interlayer spacing of ReS2 extends to about 0.98nm.

[0071] Figure 5 The Raman spectra of the samples obtained in the above examples are shown in Figure 1. The spectra of sample 1 (ReS2@C), sample 2 (rGO@ReS2@C) and sample 3 (CNT@ReS2@C) are all at 146.2 cm –1 There is a significant peak at 157.1cm –1 There is a secondary peak at , which corresponds to the in-plane vibration mode of the Re-S bond (E g ), at 206.2cm –1 The peak at corresponds to the out-of-plane vibration mode of the Re-S bond (A g ). At 1350 and 1590cm –1 There are also two broadened peaks at , corresponding to the sp3-coordinated disordered carbon (D band) and sp2-coordinated graphitized carbon (G band) of carbon materials.

[0072] In order to characterize the electrochemical performance of the samples obtained in the above examples, the following tests were performed.

[0073] Step 1: Grind the samples prepared in each embodiment with graphite and sodium carboxymethyl cellulose in a mass ratio of 6:2:2 in an agate mortar into a uniform slurry, coat the slurry on a copper foil, and then dry it in a vacuum drying oven at 80° C. for 12 hours to prepare a working electrode for a battery.

[0074] Step 2: Use metal potassium or sodium sheet as counter electrode, glass microfiber filter paper (GF / D, Whatman) as separator, 1.0M KFSI dissolved in ethylene carbonate (EC) and dimethyl carbonate (DMC) (EC:DMC=1:1Vol%) as electrolyte for potassium ion battery, 1.0M NaPF6 dissolved in diethylene glycol dimethyl ether (DEGDME) as electrolyte for sodium ion battery, and assemble CR2032 button battery in an inflatable glove box (Etelux Lab 200, O2<0.1ppm, H2O<0.1ppm).

[0075] Step 3: Use Neware's CT4008T 5V / 10mA / 50mA system to perform battery charge and discharge tests on the assembled button batteries in a voltage window of 0.01-3.00V.

[0076] Figure 6 The variable rate performance curves of potassium ion button cells assembled from sample 1 (ReS2@C), sample 2 (rGO@ReS2@C) and sample 3 (CNT@ReS2@C). Sample 2 (rGO@ReS2@C) exhibits excellent potassium storage rate performance at current densities of 0.2, 0.5, 1, 2, and 5 A g –1 The performance was 324, 290, 262, 232, and 185 mAh g –1 The discharge specific capacity shows that the ReS2 two-dimensional superlattice structure has more advantages over carbon-based materials.

[0077] Figure 7 Potassium ion button cells assembled for sample 1 (ReS2@C), sample 2 (rGO@ReS2@C) and sample 3 (CNT@ReS2@C) at a low current density of 0.5Ag –1 The specific capacity of sample 2 (rGO@ReS2@C) is 184 mAh g after 200 cycles. –1 The calculated capacity retention rate is 64.1%, showing excellent stability. Sample 1 (ReS2@C) and sample 3 (CNT@ReS2@C) have 230 mAh g –1 and 265mAh g –1 The reversible specific capacity shows an outstanding discharge specific capacity and the Coulombic efficiency (CE) during the cycle is basically maintained at 99%.

[0078] Figure 8 The long cycle performance curve of the potassium ion button battery assembled for sample 2 (rGO@ReS2@C) tested at a high current. Sample 2 at 2Ag –1 The discharge capacity of the battery in the initial cycle was 226 mAh g –1 , and maintained 107 mAh g after 300 cycles –1 The capacity of the battery is excellent, showing excellent long-term cycling ability and the Coulombic efficiency (CE) is basically maintained at 99.5%.

[0079] Fig. 9 The long cycle performance curve of the sodium ion button battery assembled for sample 2 (rGO@ReS2@C) tested at a high current. Sample 2 at 5Ag –1 The discharge capacity of the battery in the initial cycle was 288 mAh g –1, and maintained 274 mAh g after 2000 cycles –1 The capacity of the battery is excellent, showing outstanding long-term cycle stability, and its Coulombic efficiency (CE) is basically maintained at 100%.

[0080] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a ReS2 two-dimensional superlattice structure, characterized in that: The steps include: Step 1, weigh 2-6 mmol CH4N2S or C2H5NS and add it to 3-10 mL of deionized water, stir for 1-20 minutes to obtain solution A; Step 2, add 20-400 mg of carbon-based material to 15-30 mL of deionized water, ultrasonicate for 0.1-5 hours, stir for 0.1-2 hours, continue to add 0.5-1.5 mmol of NH4ReO4 and 2-6 mmol of NH3OHCl, stir for 1-40 minutes, and obtain solution B; Step 3, adding 1-6 mL of an amino compound and 0.5-8 g of a reducing sugar to the solution B in sequence, stirring for 1-20 minutes, to obtain a solution C; Step 4, quickly transferring the solution C into the solution A, sealing and stirring for 10-40 minutes to obtain a mixed solution; transferring the mixed solution into a reaction kettle and reacting at 160-220° C. for 12-24 hours to obtain an initial product; Step 5, centrifugally washing the initial product and then drying it in a vacuum drying oven to obtain an intermediate product; Step 6: Place the intermediate product in a tubular furnace, then heat it to 500-900°C in a vacuum environment, keep it warm for 1-3 hours, and finally cool it to room temperature to obtain the target product ReS2 two-dimensional superlattice structure.

2. The preparation method according to claim 1, characterized in that: The carbon-based material is one of reduced graphene oxide, carbon nanotubes, carbon cloth, carbon nanowires and carbon balls.

3. The preparation method according to claim 1, characterized in that: The amino compound is ethylenediamine.

4. The preparation method according to claim 1, characterized in that: The reducing sugar is glucose.

5. The preparation method according to claim 1, characterized in that: The cleaning in step 5 is performed by sequentially washing with deionized water and anhydrous ethanol.

6. A ReS2 two-dimensional superlattice structure obtained by the preparation method described in any one of claims 1 to 5.

7. An application of the ReS2 two-dimensional superlattice structure according to claim 6 as a negative electrode material in a potassium ion battery or a sodium ion battery.

Citation Information

Patent Citations

  • Method for preparing rhenium disulfide nanosheets

    CN106277064A

  • Preparation method of metal-doped rhenium disulfide nano-sheet array for electrocatalytic overall water splitting

    CN110508292A

  • Nano composite material, and preparation method and application thereof

    CN110838572A

  • Dual-carbon modified rhenium disulfide nanosheet as well as preparation method and application thereof

    CN116722119A

  • Nitrogen-doped single-layer amorphous carbon intercalated MoX2 nanosheet growing on carbon-based material and application of nitrogen-doped single-layer amorphous carbon intercalated MoX2 nanosheet

    CN116947103A