Lithium cobalt oxide positive electrode material and preparation method and application thereof

By forming a cladding layer on the surface of lithium cobalt oxide, the problem of poor cycling stability of lithium cobalt oxide positive electrode material under high voltage is solved, its charging and discharge capacity and thermal stability are improved, and it is suitable for high-energy density lithium-ion batteries .

CN118929775AActive Publication Date: 2024-11-12GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410769474.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-12
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The increase in the charging voltage of the existing lithium cobalt oxide positive electrode material leads to a sharp attenuation of capacity during cycling and high-temperature storage, and poor cycle stability, limiting high voltage and high specific energy applications.

Method used

By performing the first sintering treatment of lithium cobalt oxide, ammonium fluorometic acid and lithium fluoride at 600-800°C, a uniform cladding layer is formed, which reduces oxygen activity, inhibits cobalt dissolution, and improves structural stability and Cyclic performance.

Benefits of technology

It improves the charge and discharge capacity, circulation performance and thermal stability of lithium cobalt oxide positive electrode material, reduces oxygen activity, enhances structural stability and storage performance, and is suitable for high energy density lithium-ion battery applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929775A_ABST
    Figure CN118929775A_ABST
Patent Text Reader

Abstract

The invention provides a lithium cobalt oxide positive electrode material and a preparation method and application thereof, and belongs to the technical field of positive electrode materials. The preparation method of the lithium cobalt oxide positive electrode material comprises the following steps: carrying out first sintering treatment on a mixture containing lithium cobalt oxide, fluorine metal acid ammonium salt and lithium fluoride to obtain the lithium cobalt oxide positive electrode material; wherein the fluorine metal acid ammonium salt is at least two of (NH4) 2ZrF6, (NH4) 2TiF6, (NH4) 3AlF6 and (NH4) 2SnF6, and the temperature of the first sintering treatment ranges from 600 DEG C to 800 DEG C. According to the preparation method of the lithium cobalt oxide positive electrode material disclosed by the invention, the charge-discharge capacity, the cycle performance, the thermal stability and the storage performance of the battery can be improved, and the gas production performance of the battery is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of positive electrode materials, and in particular to a lithium cobalt oxide positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium cobalt oxide cathode materials are widely used in 3C electronic products due to their high compaction density. The multifunctional, miniaturized and intelligent development of 3C electronic products has put forward higher requirements for the volume energy density of lithium-ion batteries. The theoretical capacity of lithium cobalt oxide cathode materials is 274mAh / g, while the capacity of lithium cobalt oxide cathode materials currently widely used is only 140mAh / g, which means that only half of Li + Increasing the charging voltage can increase the specific capacity of the battery, but it will cause a sharp attenuation of capacity during the cycle and high-temperature storage process, and the cycle stability is extremely poor, which is also the main bottleneck restricting the application of high-voltage, high-specific-energy lithium cobalt oxide positive electrode materials. Therefore, it is urgent to develop a lithium cobalt oxide positive electrode material with high charge and discharge capacity, cycle performance and thermal stability. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a lithium cobalt oxide positive electrode material and a preparation method and application thereof.

[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a lithium cobalt oxide positive electrode material, comprising the following steps:

[0005] A mixture comprising lithium cobalt oxide, ammonium fluorometalate and lithium fluoride is subjected to a first sintering treatment to obtain a lithium cobalt oxide positive electrode material; wherein the ammonium fluorometalate is (NH 4 ) 2 ZF 6 NH 4 ) 2 TiF 6 NH 4 ) 3 AlF 6 NH 4 ) 2 S F 6 At least two of the above, the temperature of the first sintering treatment is 600-800°C.

[0006] In some embodiments, the mass of the ammonium fluorometallate salt is 1-3% of the mass of the lithium cobalt oxide.

[0007] In some embodiments, the mass of the lithium fluoride is 0.5-1.5% of the mass of the lithium cobalt oxide.

[0008] In some embodiments, the preparation method of the lithium cobalt oxide is: subjecting a mixture including the first lithium cobalt oxide, the second lithium cobalt oxide and the additive to a second sintering treatment to obtain the lithium cobalt oxide.

[0009] In some embodiments, the median particle size D of the first lithium cobalt oxide is v 50 1 The median particle size D of the second lithium cobalt oxide is 18-21 μm. v 50 2 4.5-6μm.

[0010] In some embodiments, the first lithium cobalt oxide contains a first doping metal element; optionally, the first doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr.

[0011] In some embodiments, the second lithium cobalt oxide contains a second doping metal element; optionally, the second doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr.

[0012] In some embodiments, the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 3-4:1.

[0013] In some embodiments, the mass of the additive is 2.8-4.2% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide.

[0014] In some embodiments, the additive is a compound containing a third doping metal element.

[0015] In some embodiments, the compound containing the third doping metal element includes at least one of an oxide of the third doping metal element, a hydroxide containing the third doping metal element, and an inorganic salt containing the third doping metal element.

[0016] In some embodiments, the third doping metal element includes at least one of Co, Ni, V, Mn, Al, Ti, F, Y, La, Zr, Ge, Ba, W, Nb, Cu, B, Sr, Ga, Zn, Mo, Si, and Sb.

[0017] In a second aspect, a lithium cobalt oxide positive electrode material is provided, wherein the lithium cobalt oxide positive electrode material is prepared by the preparation method of the lithium cobalt oxide positive electrode material.

[0018] In a third aspect, a positive electrode plate is provided, comprising the lithium cobalt oxide positive electrode material.

[0019] In a fourth aspect, a lithium-ion battery is provided, comprising the positive electrode plate.

[0020] In a fifth aspect, an electronic device is provided, comprising the lithium-ion battery.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The mixture of lithium cobalt oxide, ammonium fluorometalate and lithium fluoride is subjected to a first sintering treatment at a temperature of 600-800°C to form a uniform first coating layer on the surface of the lithium cobalt oxide. The first coating layer can improve the charge and discharge capacity, cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material. 4 + Heating decomposition produces NH 3 , NH 3 It reacts with lithium cobalt oxide to produce oxygen vacancies, which can reduce the O 2p orbital, reduce the overlap between the O 2p orbital and the Co 3d orbital, and reduce the oxygen activity on the surface of the lithium cobalt oxide positive electrode material; secondly, the F- in the ammonium fluorometallate salt can replace the O 2- The formation of Co-F bonds inhibits the dissolution of cobalt in the electrolyte, reduces the loss of cobalt, and improves the stability, cycle performance, and storage performance of the lithium cobalt oxide positive electrode material structure; secondly, the metal ions in the ammonium fluorometallate salt can form a metal fluoride layer on the surface of lithium cobalt oxide, inhibiting the direct contact between lithium cobalt oxide and the electrolyte, and improving the stability, cycle performance, and storage performance of the lithium cobalt oxide positive electrode material structure. Lithium fluoride can play a role in lithium supplementation and increase the capacity of lithium cobalt oxide positive electrode materials; at the same time, lithium fluoride and ammonium fluorometallate salts work synergistically to improve the charge and discharge capacity, cycle performance, thermal stability, and storage performance of lithium cobalt oxide positive electrode materials.

[0023] (2) The preparation method of the lithium cobalt oxide positive electrode material disclosed in the present invention adopts a solid phase reaction, which has a simple and easy process, low manufacturing cost, good reproducibility, and is convenient for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope image of the lithium cobalt oxide positive electrode material of Example 1;

[0025] Figure 2 This is a scanning electron microscope image of the lithium cobalt oxide positive electrode material of Comparative Example 1. DETAILED DESCRIPTION

[0026] In order to facilitate understanding of the present disclosure, the present disclosure will be described more fully below. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present disclosure more thorough and comprehensive.

[0027] For simplicity, the present disclosure only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. It should be noted that, unless otherwise stated, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.

[0029] The above application contents of the present disclosure are not intended to describe each disclosed embodiment or each implementation in the present disclosure. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of embodiments, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0030] In a first aspect of the present disclosure, a method for preparing a lithium cobalt oxide positive electrode material is provided, comprising the following steps:

[0031] S1: subjecting a mixture comprising lithium cobalt oxide, ammonium fluorometalate and lithium fluoride to a first sintering treatment to obtain a lithium cobalt oxide positive electrode material; wherein the ammonium fluorometalate is (NH 4 ) 2 ZF 6 NH 4 ) 2 TiF 6 NH 4 ) 3 AlF 6 NH 4 ) 2 S F 6 At least two of the following; the temperature of the first sintering treatment is 600-800°C, for example, it can be but not limited to 600°C, 650°C, 700°C, 750°C, 800°C.

[0032] In step S1, ammonium fluorometallate and lithium fluoride are added, and sintering treatment is performed at a temperature of 600-800°C, so that a uniform first coating layer can be formed on the surface of lithium cobalt oxide. The first coating layer can improve the charge and discharge capacity, cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material.

[0033] NH in ammonium fluorometallate salts 4 + Heating decomposition produces NH 3 , NH 3 It reacts with lithium cobalt oxide to produce oxygen vacancies, which can reduce the O 2p orbital, reduce the overlap between the O 2p orbital and the Co 3d orbital, and reduce the oxygen activity on the surface of the lithium cobalt oxide positive electrode material; secondly, the F- in the ammonium fluorometallate salt can replace the O 2- The formation of Co-F bonds inhibits the dissolution of cobalt in the electrolyte, reduces the loss of cobalt, and improves the stability of the structure, cycle performance and storage performance of the lithium cobalt oxide positive electrode material; secondly, the metal ions in the ammonium fluorometallate salt can form a metal fluoride layer on the surface of lithium cobalt oxide, inhibiting the direct contact between lithium cobalt oxide and the electrolyte, and improving the stability of the structure, cycle performance and storage performance of the lithium cobalt oxide positive electrode material.

[0034] Lithium fluoride can supplement lithium and increase the capacity of lithium cobalt oxide positive electrode materials; at the same time, lithium fluoride and ammonium fluorometallate salts work synergistically to improve the charge and discharge capacity, cycle performance, thermal stability and storage performance of lithium cobalt oxide positive electrode materials.

[0035] The temperature of the first sintering treatment is within the above range, which can improve the charge and discharge capacity, cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material; if the temperature of the first sintering treatment is <600°C, the ammonium fluorometallate salt is not fully decomposed, resulting in a decrease in the charge and discharge capacity, cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material; if the temperature of the first sintering treatment is >800°C, an irreversible phase change will occur on the surface of the lithium cobalt oxide positive electrode material to generate a rock salt stone phase, resulting in a decrease in the charge and discharge capacity, cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material.

[0036] It should be noted that the "lithium cobalt oxide" and "lithium cobalt oxide" mentioned in this disclosure are not limited to LiCoO 2 As long as it is an oxide containing lithium and cobalt elements, for example, an oxide containing lithium and cobalt elements doped with other metal elements (such as transition metal elements), it is within the protection scope of the present disclosure.

[0037] In some embodiments, the first sintering treatment time is 5-8 hours, for example, but not limited to 5 hours, 6 hours, 7 hours, and 8 hours.

[0038] In some embodiments, the mass of the ammonium fluorometallate salt is 1-3% of the mass of the lithium cobalt oxide, for example, but not limited to 1%, 1.2%, 1.5%, 2%, 2.5%, 2.7%, 3%.

[0039] In some embodiments, the mass of the lithium fluoride is 0.5-1.5% of the mass of the lithium cobalt oxide, for example, it can be but not limited to 0.5%, 0.8%, 1%, 1.2%, 1.5%.

[0040] Adding the above-mentioned amount of ammonium fluorometallate and lithium fluoride in step S1 can make the first coating layer reach an appropriate thickness. Therefore, when the lithium cobalt oxide positive electrode material is used in a battery, it can effectively resist the corrosion of the lithium cobalt oxide positive electrode material by the electrolyte byproducts and reduce the dissolution of the transition metal. At the same time, it can avoid the first coating layer being too thick to affect ion transmission, thereby improving the capacity, cycle performance, storage performance and thermal stability of the lithium cobalt oxide positive electrode material.

[0041] If the addition amount of ammonium fluorometallate and lithium fluoride is too high, the obtained first coating layer will be relatively thick, which will affect ion transport and cause the capacity of the lithium cobalt oxide positive electrode material to decrease; if the addition amount of ammonium fluorometallate and lithium fluoride is too small, the obtained first coating layer will be relatively thin, which is not conducive to resisting the corrosion of the lithium cobalt oxide positive electrode material by the electrolyte by-products, resulting in a decrease in the cycle performance, thermal stability and storage performance of the lithium cobalt oxide positive electrode material.

[0042] In the present disclosure, the median particle size D of the lithium cobalt oxide v 50 5 It is 16-18μm, for example, it can be but not limited to 16μm, 16.5μm, 17μm, 17.5μm, 18μm.

[0043] In some embodiments, the present disclosure also includes a method for preparing lithium cobalt oxide, comprising the following steps: S2: subjecting a mixture comprising a first lithium cobalt oxide, a second lithium cobalt oxide, and an additive to a second sintering treatment to obtain lithium cobalt oxide.

[0044] In some embodiments, the median particle size D of the first lithium cobalt oxide is v 50 1 The median particle size D of the second lithium cobalt oxide is 18-21 μm, for example, but not limited to 18 μm, 18.5 μm, 19 μm, 19.5 μm, 20 μm, 20.5 μm, 21 μm; v 50 2 It is 4.5-6μm, for example, it can be but not limited to 4.5μm, 4.8μm, 5.0μm, 5.2μm, 5.5μm, 5.7μm, and 6μm.

[0045] The median particle size D of the first lithium cobalt oxidev 50 1 The median particle size D of the second lithium cobalt oxide v 50 2 Being within the above range, a combination of large particles and small particles can be formed in the lithium cobalt oxide positive electrode material, which is beneficial to improving the compaction density of the lithium cobalt oxide positive electrode material.

[0046] In some embodiments, the first lithium cobalt oxide comprises a first doping metal element; optionally, the first doping metal element comprises at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr;

[0047] In some embodiments, the second lithium cobalt oxide comprises a second doping metal element; optionally, the second doping metal element comprises at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr;

[0048] In some embodiments, the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 3-4:1, for example, but not limited to, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1.

[0049] The mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is within the above range, which is beneficial to improving the compaction density of the lithium cobalt oxide positive electrode material and improving the volume energy density of the battery. If the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is greater than 4:1, it is easy to cause the charge and discharge capacity of the battery to deteriorate.

[0050] In some embodiments, the mass of the additive is 2.8-4.2% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide, for example, but not limited to 2.8%, 3.0%, 3.2%, 3.4%, 3.5%, 3.8%, 4.0%, 4.2%.

[0051] Adding the additive in the above-mentioned amount in step S2 can form a thin and uniform second coating layer on the partial surface of the first lithium cobalt oxide and the second lithium cobalt oxide. The second coating layer can promote the increase of the thermal stability of the positive electrode material, thereby improving the high-temperature cycle stability of the lithium-ion battery.

[0052] In some embodiments, the additive is a compound containing a third doping metal element;

[0053] In some embodiments, the compound containing the third doping metal element includes at least one of an oxide of the third doping metal element, a hydroxide containing the third doping metal element, and an inorganic salt containing the third doping metal element;

[0054] In some embodiments, the third doping metal element includes at least one of Co, Ni, V, Mn, Al, Ti, F, Y, La, Zr, Ge, Ba, W, Nb, Cu, B, Sr, Ga, Zn, Mo, Si, and Sb.

[0055] The second coating layer contains a third doped metal element, which is beneficial to further inhibit the direct contact between lithium cobalt oxide and the electrolyte, further inhibit the dissolution of cobalt in the electrolyte, reduce the loss of cobalt, and improve the stability of the positive electrode material structure, thereby further improving the cycle performance of the battery.

[0056] In some embodiments, the temperature of the second sintering treatment is 900-950°C, for example, but not limited to, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C.

[0057] In some embodiments, the second sintering treatment time is 6-10 hours, for example, but not limited to 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours.

[0058] In some embodiments, the present disclosure also includes a method for preparing a first lithium cobalt oxide, comprising the following steps:

[0059] A mixture including a first lithium source and a first cobalt source is subjected to a first calcination treatment to obtain a first lithium cobalt oxide.

[0060] In some embodiments, the temperature of the first calcination treatment is 1050-1100°C, for example, but not limited to, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C.

[0061] In some embodiments, the time of the first calcination treatment is 8-12 hours, for example, but not limited to, 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours.

[0062] In some embodiments, the molar ratio of the lithium element in the first lithium source to the cobalt element in the first cobalt source is 1.07-1.09, for example, but not limited to 1.07, 1.075, 1.08, 1.085, 1.09.

[0063] The molar ratio of lithium to cobalt is within the above range, which can make the residual alkali, pH value, particle size, tap density and compacted density in the first lithium cobalt oxide all within a suitable and preferred range. If the molar ratio of lithium to cobalt exceeds the above range, it is easy to cause the residual alkali, pH value and other parameters to be high, and ultimately it is easy to cause the cycle performance of the lithium cobalt oxide positive electrode material to decrease.

[0064] In some embodiments, the median particle size D of the first cobalt source is v 503 It is 13.5-18.5μm, for example, it can be but not limited to 13.5μm, 14μm, 15μm, 16μm, 17μm, 18.5μm.

[0065] In some embodiments, the mixture comprising the first lithium source and the first cobalt source further comprises a compound comprising a first doping metal element.

[0066] In some embodiments, the mass of the compound containing the first doping metal element is 0.3-3.5% of the mass of the first cobalt source, for example, but not limited to 0.3%, 0.5%, 1%, 1.5%, 2%, 2.5%, 2.8%, 3%.

[0067] In some embodiments, the first doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr.

[0068] In some embodiments, the present disclosure also includes a method for preparing a second lithium cobalt oxide, comprising the following steps:

[0069] The mixture including the second lithium source and the second cobalt source is subjected to a second calcination treatment to obtain a second lithium cobalt oxide.

[0070] In some embodiments, the temperature of the second calcination treatment is 1000-1050°C, for example, it can be but not limited to 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C.

[0071] In some embodiments, the second calcination treatment time is 8-12 hours, for example, but not limited to 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours.

[0072] In some embodiments, the molar ratio of the lithium element in the second lithium source to the cobalt element in the second cobalt source is 1.07-1.09, for example, but not limited to 1.07, 1.075, 1.08, 1.085, 1.09.

[0073] The molar ratio of lithium to cobalt is within the above range, which can make the residual alkali, pH value, particle size, tap density and compacted density in the second lithium cobalt oxide all within a suitable and preferred range. If the molar ratio of lithium to cobalt exceeds the above range, it is easy to cause the residual alkali, pH value and other parameters to be high, and ultimately it is easy to cause the cycle performance of the lithium cobalt oxide positive electrode material to decrease.

[0074] In some embodiments, the median particle size D of the second cobalt source is v 50 4It is 1.5-6.5μm, for example, it can be but not limited to 1.5μm, 2μm, 3μm, 4μm, 5μm, 6μm, and 6.5μm.

[0075] In some embodiments, the mixture comprising the second lithium source and the second cobalt source further comprises a compound comprising a second doping metal element.

[0076] In some embodiments, the mass of the compound containing the second doping metal element is 0.2-1.6% of the mass of the second cobalt source, for example, but not limited to 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%.

[0077] In some embodiments, the second doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr.

[0078] In some embodiments, the first lithium source and the second lithium source are each independently at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxide, lithium chloride, lithium bromide and lithium fluoride.

[0079] In some embodiments, the first cobalt source and the second cobalt source are each independently at least one of cobalt trioxide, cobalt hydroxide, cobaltous oxide, cobalt nitrate, cobalt sulfate, and cobalt oxyhydroxide.

[0080] In this disclosure, the median particle size D v 50 can be obtained by testing with a laser particle size analyzer.

[0081] In a second aspect, a lithium cobalt oxide positive electrode material is provided, wherein the lithium cobalt oxide positive electrode material is prepared by the preparation method of the lithium cobalt oxide positive electrode material described in the first aspect.

[0082] In a third aspect, a positive electrode plate is provided, comprising the lithium cobalt oxide positive electrode material described in the second aspect.

[0083] In a fourth aspect, a lithium-ion battery is provided, comprising the positive electrode sheet described in the third aspect.

[0084] In some embodiments, the lithium-ion battery further includes a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, lithium ions are inserted and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0085] In a fifth aspect, an electronic device is provided, comprising the lithium-ion battery described in the fourth aspect.

[0086] In some embodiments, the type of electronic device is not particularly limited, and it can be any electronic device known in the prior art. For example, the electronic device can include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, etc.

[0087] Example 1

[0088] A method for preparing a lithium cobalt oxide positive electrode material comprises the following steps:

[0089] (1) D v Cobaltous oxide with a diameter of 15.5 μm, lithium carbonate and a compound containing a first doping element are uniformly mixed to obtain a first mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the first doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the first doping element is 2.3% of the mass of cobaltous oxide; the first mixture is sintered in a high-temperature box furnace at 1070° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 was 18.8 μm, and the first lithium cobalt oxide was obtained.

[0090] (2) D v 50 is 3.2 μm cobalt tetroxide, lithium carbonate and a compound containing a second doping element are uniformly mixed to obtain a second mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the second doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the second doping element is 1.2% of the mass of cobalt tetroxide; the second mixture is sintered in a high-temperature box furnace at 1020° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 is 5.5 μm, and a second lithium cobalt oxide is obtained.

[0091] (3) mixing the first lithium cobalt oxide, the second lithium cobalt oxide and the additive uniformly to obtain a third mixture; wherein the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 4:1, the additive is aluminum oxide, lanthanum oxide, yttrium oxide, zinc oxide and zirconium oxide mixed in a mass ratio of 1:1:1:1:1, and the mass of the additive is 3.5% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide; sintering the third mixture in a high-temperature box furnace at 920° C. in an air atmosphere for 8 h, cooling, and crushing to D v 50 is 16.5 μm, and the third lithium cobalt oxide is obtained.

[0092] (4) uniformly mixing the third lithium cobalt oxide, the fluorometallic acid ammonium salt and lithium fluoride to obtain a fourth mixture, wherein the fluorometallic acid ammonium salt is (NH 4 ) 2 ZF6 NH 4 ) 2 TiF 6 The fourth mixture is mixed in a mass ratio of 1:1, wherein the mass of the ammonium fluorometallate salt is 2% of the mass of the lithium cobalt oxide, and the mass of the lithium fluoride is 1% of the mass of the lithium cobalt oxide; the fourth mixture is sintered in a high-temperature box furnace at 700°C in an air atmosphere for 6 hours, and cooled to obtain a lithium cobalt oxide positive electrode material.

[0093] Example 2

[0094] A method for preparing a lithium cobalt oxide positive electrode material comprises the following steps:

[0095] (1) D v Cobaltous oxide with a diameter of 13.5 μm, lithium carbonate and a compound containing a first doping element are uniformly mixed to obtain a first mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the first doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the first doping element is 0.3% of the mass of cobaltous oxide; the first mixture is sintered in a high-temperature box furnace at 1050° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 was 18.1 μm, and the first lithium cobalt oxide was obtained.

[0096] (2) D v 50 is 1.6 μm cobalt tetroxide, lithium carbonate and a compound containing a second doping element are uniformly mixed to obtain a second mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the second doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the second doping element is 0.2% of the mass of cobalt tetroxide; the second mixture is sintered in a high-temperature box furnace at 1020° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 is 4.5 μm, and a second lithium cobalt oxide is obtained.

[0097] (3) mixing the first lithium cobalt oxide, the second lithium cobalt oxide and the additive uniformly to obtain a third mixture; wherein the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 3:1, the additive is aluminum oxide, lanthanum oxide, yttrium oxide, zinc oxide and zirconium oxide mixed in a mass ratio of 1:1:1:1:1, and the mass of the additive is 2.8% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide; sintering the third mixture in a high-temperature box furnace at 920° C. in an air atmosphere for 8 h, cooling, and crushing to D v 50 is 16.5 μm, and the third lithium cobalt oxide is obtained.

[0098] (4) uniformly mixing the third lithium cobalt oxide, the fluorometallic acid ammonium salt and lithium fluoride to obtain a fourth mixture, wherein the fluorometallic acid ammonium salt is (NH 4 ) 2 ZF 6 and (NH 4 ) 2 AlF 6 The fourth mixture is mixed in a mass ratio of 1:1, wherein the mass of the ammonium fluorometallate salt is 1% of the mass of the lithium cobalt oxide, and the mass of the lithium fluoride is 0.5% of the mass of the lithium cobalt oxide; the fourth mixture is sintered in a high-temperature box furnace at 700°C in an air atmosphere for 6 hours, and cooled to obtain a lithium cobalt oxide positive electrode material.

[0099] Example 3

[0100] A method for preparing a lithium cobalt oxide positive electrode material comprises the following steps:

[0101] (1) D v Cobaltous oxide with a diameter of 18.4 μm, lithium carbonate and a compound containing a first doping element are uniformly mixed to obtain a first mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the first doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the first doping element is 3.5% of the mass of cobaltous oxide; the first mixture is sintered in a high-temperature box furnace at 1050° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 was 20.9 μm, and the first lithium cobalt oxide was obtained.

[0102] (2) D v Cobaltous oxide with a diameter of 6.3 μm, lithium carbonate and a compound containing a second doping element are uniformly mixed to obtain a second mixture; wherein the molar ratio of lithium to cobalt is 1.08, the compound containing the second doping element is a mixture of magnesium oxide, aluminum oxide and titanium oxide in a mass ratio of 1:1:1, and the mass of the compound containing the second doping element is 1.6% of the mass of cobaltous oxide; the second mixture is sintered in a high-temperature box furnace at 1020° C. in an air atmosphere for 10 hours, cooled, and crushed to D v 50 was 5.8 μm, and a second lithium cobalt oxide was obtained.

[0103] (3) uniformly mixing the first lithium cobalt oxide, the second lithium cobalt oxide and the additive to obtain a third mixture; wherein the mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 3.5:1, the additive is aluminum oxide, lanthanum oxide, yttrium oxide, zinc oxide and zirconium oxide mixed in a mass ratio of 1:1:1:1:1, and the mass of the additive is 4.2% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide; sintering the third mixture in a high-temperature box furnace at 920° C. in an air atmosphere for 8 h, cooling, and crushing to D v50 is 17.8 μm, and the third lithium cobalt oxide is obtained.

[0104] (4) uniformly mixing the third lithium cobalt oxide, the fluorometallic acid ammonium salt and lithium fluoride to obtain a fourth mixture, wherein the fluorometallic acid ammonium salt is (NH 4 ) 2 ZF 6 and (NH 4 ) 2 S F 6 The mixture is mixed in a mass ratio of 1:1, wherein the mass of the ammonium fluorometallate salt is 3% of the mass of the lithium cobalt oxide, and the mass of the lithium fluoride is 1.5% of the mass of the lithium cobalt oxide; the fourth mixture is sintered in a high-temperature box furnace at 700°C in an air atmosphere for 6 hours, and cooled to obtain a lithium cobalt oxide positive electrode material.

[0105] Example 4

[0106] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in embodiment 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this embodiment is (NH 4 ) 2 TiF 6 and (NH 4 ) 2 AlF 6 The mixture was mixed in a mass ratio of 1:1, and the remaining steps and parameters were the same as those in Example 1.

[0107] Example 5

[0108] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in embodiment 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this embodiment is (NH 4 ) 2 TiF 6 and (NH 4 ) 2 S F 6 The mixture was mixed in a mass ratio of 1:1, and the remaining steps and parameters were the same as those in Example 1.

[0109] Example 6

[0110] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in embodiment 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this embodiment is (NH 4 ) 2 ZF 6 NH 4 ) 2 TiF 6 and (NH 4 ) 2 AlF 6The mixture was mixed in a mass ratio of 1:1:1, and the remaining steps and parameters were the same as those in Example 1.

[0111] Example 7

[0112] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in embodiment 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this embodiment is (NH 4 ) 2 TiF 6 NH 4 ) 2 AlF 6 and (NH 4 ) 2 S F 6 The mixture was mixed in a mass ratio of 1:1:1, and the remaining steps and parameters were the same as those in Example 1.

[0113] Example 8

[0114] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in embodiment 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this embodiment is (NH 4 ) 2 ZF 6 NH 4 ) 2 TiF 6 NH 4 ) 2 AlF 6 and (NH 4 ) 2 S F 6 The mixture was mixed in a mass ratio of 1:1:1:1, and the remaining steps and parameters were the same as those in Example 1.

[0115] Example 9

[0116] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in Embodiment 1 only in that the sintering temperature in step (4) is 600° C., and the remaining steps and parameters are the same as those in Embodiment 1.

[0117] Example 10

[0118] The preparation method of the lithium cobalt oxide positive electrode material in this embodiment is different from that in Embodiment 1 only in that the sintering temperature in step (4) is 800° C., and the remaining steps and parameters are the same as those in Embodiment 1.

[0119] Comparative Example 1

[0120] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that step (4) is not performed, that is, the third lithium cobalt oxide is the lithium cobalt oxide positive electrode material in this comparative example, and the remaining steps and parameters are the same as those in Example 1.

[0121] Comparative Example 2

[0122] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that the ammonium fluorometallate salt in step (4) is different. The ammonium fluorometallate salt in this comparative example is (NH 4 ) 2 ZF 6 , the remaining steps and parameters are the same as those in Example 1.

[0123] Comparative Example 3

[0124] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that lithium fluoride is not added in step (4), and the remaining steps and parameters are the same as those in Example 1.

[0125] Comparative Example 4

[0126] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that no ammonium fluorometallate salt is added in step (4), and the remaining steps and parameters are the same as those in Example 1.

[0127] Comparative Example 5

[0128] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that the sintering temperature in step (4) is 400° C., and the remaining steps and parameters are the same as those in Example 1.

[0129] Comparative Example 6

[0130] The preparation method of the lithium cobalt oxide positive electrode material in this comparative example is different from that in Example 1 only in that the sintering temperature in step (4) is 900° C., and the remaining steps and parameters are the same as those in Example 1.

[0131] Performance Testing

[0132] 1. The lithium cobalt oxide positive electrode material prepared in the embodiment and the comparative example is used as the positive electrode active material, and the conductive carbon and vinylidene fluoride are mixed in deionized water at a mass ratio of 95:2:3, and then coated on aluminum foil. After vacuum drying, the pressed sheet is taken out and cut into a positive electrode sheet of the required size as the positive electrode of the battery, and the lithium sheet is used as the negative electrode of the battery. The button half-cell is assembled in a glove box with oxygen and water content less than 1ppm. The assembled button half-cell is used for charge and discharge capacity test, with a test voltage of 2.3-4.55V and a current density of 1 / 3C.

[0133] 2. The lithium cobalt oxide positive electrode materials prepared in the embodiment and the comparative example were respectively used as positive electrode active materials, and were mixed evenly with conductive carbon and vinylidene fluoride in a mass ratio of 95:2:3 in deionized water, and then coated on aluminum foil. After vacuum drying, the pressed sheets were taken out and cut into positive electrode sheets of the required size as battery positive electrodes;

[0134] Anode slurry is prepared by using artificial graphite as the negative electrode active material, and the mixture is mixed evenly with conductive carbon and vinylidene fluoride in a mass ratio of 95:2:3 in deionized water, and then coated on aluminum foil. After vacuum drying, the pressed sheet is taken out and cut into anode sheets of a required size as the battery cathode;

[0135] 1 mol / L LiPF 6 The electrolyte solution was dissolved in a mixed solvent of ethylene carbonate / diethyl carbonate (volume ratio of 1:1), and 3 wt % of fluoroethylene carbonate was added and mixed evenly to obtain an electrolyte solution;

[0136] The soft pack battery is assembled from the above-mentioned positive electrode sheet, negative electrode sheet, PP / PE / PP composite film between the positive and negative electrode sheets and the above-mentioned electrolyte. The assembled soft pack battery is used to test the cycle performance, thermal stability, storage performance and gas production performance.

[0137] The cycle performance test process is as follows: the soft-pack battery is cycled for 100 weeks at 25°C with a charge and discharge current of 1C in the voltage range of 2.3-4.5V to test the battery capacity retention rate.

[0138] The thermal stability test process is as follows: the soft-pack battery is cycled for 100 weeks at 45°C with a charge and discharge current of 1C in the voltage range of 2.3-4.5V to test the battery capacity retention rate.

[0139] The storage performance test process is as follows: store the fully charged battery in a 45°C constant temperature box, test the recovery capacity every 15 days and store it again with full charge.

[0140] The gas production performance test process is as follows: store the fully charged battery in a 70°C constant temperature box, test the battery cell volume every day, and fully charge it once every 7 days.

[0141] Table 1

[0142]

[0143] It can be seen from the experimental data in Table 1 that the lithium cobalt oxide positive electrode material disclosed in the present invention can improve the charge and discharge capacity, cycle performance, thermal stability and storage performance of the battery, and reduce the gas production performance of the battery.

[0144] By comparing Example 1 and Comparative Examples 1-4, it can be seen that when at least one of ammonium fluorometallate and lithium fluoride is missing, the charge and discharge capacity, cycle performance, thermal stability and storage performance of the battery are significantly reduced, and the gas production performance is significantly increased; when only one ammonium fluorometallate is added, the charge and discharge capacity of the battery is reduced, and the gas production performance of the battery is increased, indicating that the ammonium fluorometallate and lithium fluoride disclosed in the present invention have a synergistic effect.

[0145] By comparing Example 1, Examples 9-10 and Comparative Examples 5-6, it can be seen that when the sintering temperature is lower than 600°C or higher than 800°C, the charge and discharge capacity, cycle performance, thermal stability and storage performance will decrease, and the gas production performance of the battery will increase.

[0146] Figure 1 This is a scanning electron microscope image of the lithium cobalt oxide positive electrode material of Example 1; Figure 2 This is a scanning electron microscope image of the lithium cobalt oxide positive electrode material of Comparative Example 1. Figure 1 and Figure 2 It can be seen that the surface of the material obtained in Example 1 has obvious small particles attached, while the surface of the material obtained in Comparative Example 1 is smoother.

[0147] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a lithium cobalt oxide positive electrode material, It is characterized in that The following steps are involved: A mixture comprising lithium cobalt oxide, ammonium fluorometalate and lithium fluoride is subjected to a first sintering treatment to obtain a lithium cobalt oxide positive electrode material; wherein the ammonium fluorometalate is (NH 4 ) 2 ZF 6 NH 4 ) 2 TiF 6 NH 4 ) 3 AlF 6 NH 4 ) 2 S F 6 At least two of the above, the temperature of the first sintering treatment is 600-800°C.

2. The method for preparing the lithium cobalt oxide positive electrode material according to claim 1, It is characterized in that The mass of the ammonium fluorometallate salt is 1-3% of the mass of the lithium cobalt oxide; and / or the mass of the lithium fluoride is 0.5-1.5% of the mass of the lithium cobalt oxide.

3. The method for preparing the lithium cobalt oxide positive electrode material according to claim 1, It is characterized in that The preparation method of the lithium cobalt oxide comprises: subjecting a mixture including a first lithium cobalt oxide, a second lithium cobalt oxide and an additive to a second sintering treatment to obtain the lithium cobalt oxide.

4. The method for preparing the lithium cobalt oxide positive electrode material according to claim 3, It is characterized in that The median particle size D of the first lithium cobalt oxide v 50 1 The median particle size D of the second lithium cobalt oxide is 18-21 μm. v 50 2 4.5-6μm.

5. The method for preparing the lithium cobalt oxide positive electrode material according to claim 3, It is characterized in that At least one of the following conditions is met: (1) The first lithium cobalt oxide contains a first doping metal element; optionally, the first doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr; (2) The second lithium cobalt oxide contains a second doping metal element; optionally, the second doping metal element includes at least one of Ca, Zn, Ti, Fe, Mg, Al, Y, La, and Zr; (3) The mass ratio of the first lithium cobalt oxide to the second lithium cobalt oxide is 3-4:1; (4) The mass of the additive is 2.8-4.2% of the total mass of the first lithium cobalt oxide and the second lithium cobalt oxide.

6. The method for preparing the lithium cobalt oxide positive electrode material according to claim 3, It is characterized in that The additive is a compound containing a third doping metal element; Optionally, the compound containing the third doping metal element includes at least one of an oxide of the third doping metal element, a hydroxide containing the third doping metal element, and an inorganic salt containing the third doping metal element; Further optionally, the third doping metal element includes at least one of Co, Ni, V, Mn, Al, Ti, F, Y, La, Zr, Ge, Ba, W, Nb, Cu, B, Sr, Ga, Zn, Mo, Si, and Sb.

7. A lithium cobalt oxide positive electrode material, It is characterized in that The lithium cobalt oxide positive electrode material is prepared by the preparation method of the lithium cobalt oxide positive electrode material according to any one of claims 1 to 6.

8. A positive electrode sheet, It is characterized in that Comprising the lithium cobalt oxide positive electrode material as described in claim 7.

9. A lithium ion battery, It is characterized in that Comprising the positive electrode sheet as described in claim 8.

10. An electronic device, It is characterized in that Comprising the lithium ion battery as claimed in claim 9.

Citation Information

Patent Citations

  • Method for coating nickel cobalt lithium manganate positive-electrode material with calcium fluophosphate

    CN103367723A

  • Germanium / fluorine / nitrogen co-doped lithium nickel cobalt manganate ternary positive electrode material and preparation method thereof

    CN111653762A

  • Fluorine-aluminum co-doped lithium cobalt oxide positive electrode material and preparation method thereof

    CN114695862A

  • Modification method of high-nickel positive electrode material, positive electrode material, positive electrode plate and lithium battery