Conical and hexagonal layered cobalt hydroxide nano-composite structure and preparation method thereof

Conical and hexagonal layered cobalt hydroxide nanocomposite structures were prepared by hydrothermal method and electrochemical reconstruction method, which solved the problem of single structure of nano-cobalt hydroxide and achieved better electrochemical performance and energy storage capacity.

CN118929777APending Publication Date: 2024-11-12LIAONING INST OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410963985.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing nano-cobalt hydroxide has a single structure and is difficult to synthesize in a controllable manner. There is a lack of reports on composite structures, which affects its electrochemical performance in supercapacitors.

Method used

Conical and hexagonal layered cobalt hydroxide nanocomposite structures were prepared using a hydrothermal method and an electrochemical reconstruction method. Vanadium-doped cobalt tetroxide was grown on a nickel foam substrate, and the thickness and surface roughness of the hexagonal cobalt hydroxide sheets were controlled by cyclic voltammetry for electrochemical scanning.

Benefits of technology

The controllable synthesis of conical and hexagonal layered cobalt hydroxide nanocomposites was achieved, which significantly improved their energy storage capacity and electrochemical performance in supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929777A_ABST
    Figure CN118929777A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic nano material preparation, and particularly relates to a conical and hexagonal layered cobalt hydroxide nano composite structure and a preparation method thereof. According to the method, a weak base solution containing cobalt ions, vanadium ions and a precipitator is used as a raw material, and vanadium-doped cobalt hydroxide is synthesized on a foamed nickel substrate through a hydrothermal reaction; carrying out annealing treatment to obtain foamed nickel / vanadium doped cobaltosic oxide; and taking the cobalt hydroxide nano-composite material as a working electrode to repeatedly perform electrochemical scanning in a potassium hydroxide solution, and dissolving doped vanadium in alkali liquor under the electrochemical action to induce surface reconstruction of the material, so as to obtain the conical and hexagonal layered cobalt hydroxide nano-composite structure. The composite structure is formed by compounding a conical structure with a thin top end, a thick bottom end and a rough surface and a hexagonal sheet structure which is formed by stacking a plurality of thin sheet layers with rough surfaces and layered structures, has excellent electrochemical performance, and has a good application prospect in the field of supercapacitors as an electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic nano material preparation, and in particular relates to a cone-shaped and hexagonal layered cobalt hydroxide nano composite structure and a preparation method thereof. Background Art

[0002] In the context of the current shortage of fossil energy, environmental pollution and global warming, it is urgent to vigorously develop new energy storage devices based on chemical energy such as secondary batteries and supercapacitors. In order to improve the energy storage efficiency of supercapacitors, the development of various types of electrode materials, including regulating the micromorphology and composition of materials, building composite structures, and preparing composite materials, has become a hot research direction in the current materials and energy storage fields. Among many transition metal hydroxides, cobalt hydroxide has attracted much attention due to its excellent electrochemical properties. Different types of cobalt hydroxide-based electrode materials have been developed for the preparation of high-performance supercapacitors.

[0003] At present, many nanostructured cobalt hydroxides have been synthesized for electrochemical energy storage. For example, Zhang Hongyu et al. reported a method for preparing hexagonal β-Co(OH)2 (Material Guide 2017), specifically using sodium hydroxide and hydrazine hydrate as alkaline precipitants to directly obtain tens of nanometers thick flake hexagonal β-Co(OH)2 through precipitation reaction. Tian Zhengfang et al. reported a method for preparing thin flaky calcium-doped cobalt hydroxide in patent application number 201710144721.3, specifically mixing a certain concentration of calcium hydroxide and a certain concentration of cobalt ion solution to undergo ion exchange reaction, filtering and stirring the product, and drying to prepare calcium-doped cobalt hydroxide. Wu Zhengcui et al. used copper salt, cobalt salt, hexamethylenetetramine and other raw materials to dissolve in a mixture of water and methanol in patent application number 202010531881.5, added nickel foam and carried out solvent thermal reaction in the reactor, and finally prepared a Cu-doped Co(OH)2 nanosheet array structure. In the patent application number 201510232459.9, Li Zhiying et al. added a precipitant solution containing an alkali and a nitrogen-containing ligand to a cobalt salt solution to prepare cobalt hydroxide with a hexagonal sheet structure through a precipitation reaction. In summary, the existing synthesis of cobalt hydroxide mostly adopts chemical precipitation, hydrothermal or solvothermal methods, and most of them are single-sheet cobalt hydroxide nanosheets. There are few reports on the synthesis of cobalt hydroxide nanosheets by electrochemical methods. In addition, there are few reports on cobalt hydroxide nanocomposite structures in existing patents and literature. Summary of the invention

[0004] In order to solve the problems of single structure and controllable synthesis of existing nano-cobalt hydroxide, firstly, the purpose of the present invention is to provide a conical and hexagonal layered cobalt hydroxide nano-composite structure; secondly, the purpose of the present invention is to provide a preparation method of the conical and hexagonal layered cobalt hydroxide nano-composite structure.

[0005] The conical and hexagonal layered cobalt hydroxide nanocomposite structure of the present invention is composed of a conical structure and a layered structure; the conical structure is thin at the top, thick at the bottom and has a rough surface; the layered structure has a rough surface and a layered structure, and is composed of a plurality of thin layers stacked;

[0006] The layered structure has a thickness of 150 nm to 820 nm.

[0007] The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure of the present invention comprises the following steps:

[0008] S1 preparation of vanadium-doped cobalt hydroxide: using a weak alkaline solution containing cobalt ions, vanadium ions and a precipitant as a raw material, synthesizing vanadium-doped cobalt hydroxide on a foamed nickel substrate through a hydrothermal reaction;

[0009] S2: Preparation of vanadium-doped cobalt oxide: thermally annealing the vanadium-doped cobalt hydroxide prepared in S1 to obtain foamed nickel / vanadium-doped cobalt oxide;

[0010] S3 electrochemical reconstruction of cobalt hydroxide: The nickel foam / vanadium-doped cobalt tetroxide prepared in S2 is used as the working electrode, and electrochemical scanning is repeated in a potassium hydroxide solution. Under the electrochemical action, the doped vanadium dissolves in the alkaline solution to induce surface reconstruction of the material, thereby obtaining the conical and hexagonal layered cobalt hydroxide nanocomposite structure described in the present invention.

[0011] The molar ratio of cobalt ions to vanadium ions in step S1 is V / Co<0.5;

[0012] Step S1: the cobalt ions are from strong acid salts of cobalt, including one of cobalt nitrate, cobalt chloride and cobalt sulfate; the vanadium ions are from one of vanadium chloride and vanadium sulfate; the precipitant includes urea and ammonium fluoride;

[0013] The hydrothermal reaction temperature in step S1 is 110-130°C, and the reaction time is 8-24h; the pH of the weak alkaline solution is 8-10;

[0014] The annealing treatment temperature in step S2 is 200-400° C. and the treatment time is 3-10 hours;

[0015] The electrochemical scanning in step S3 specifically adopts cyclic voltammetry, with a scanning speed of 1 to 8 mV / s and a number of repeated scanning cycles of 5 to 300 cycles; the concentration of the potassium hydroxide solution is 1 to 6 mol / L.

[0016] The electrode material of the conical and hexagonal layered cobalt hydroxide nanocomposite structure described in the present invention has a good application prospect in the field of supercapacitors. Compared with the prior art, the characteristics and beneficial effects of the present invention are:

[0017] (1) The present invention grows vanadium-doped cobalt oxide as a template on the surface of a nickel foam substrate, and prepares a rough surface conical and thick hexagonal layered cobalt hydroxide nanocomposite structure by an electrochemical method. Different from the traditional chemical precipitation method and electrochemical deposition method, this method can control the number of electrochemical scanning cycles to adjust the thickness of the hexagonal cobalt hydroxide sheet layer, thereby realizing the controllable synthesis of the nanocomposite structure.

[0018] (2) Compared with the single-structure cobalt hydroxide reported so far, including nanosheets and nanoparticles, this nanocomposite structure containing conical and hexagonal layers has a rough surface and is composed of several stacked thin layers. It can give full play to the advantages and synergistic effects of the conical and lamellar structures, show better electrochemical properties, and further improve the energy storage capacity of the electrode material in the supercapacitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the morphology of vanadium-doped cobalt hydroxide prepared in Example 1.

[0020] Figure 2 This is the XRD pattern of the pyramidal and hexagonal layered cobalt hydroxide nanocomposite structure prepared in Example 1.

[0021] Figure 3 This is the morphology of the conical and hexagonal layered cobalt hydroxide nanocomposite structure prepared in Example 1.

[0022] Figure 4 (a) and Figure 4 (b) are morphology images of the conical and hexagonal layered cobalt hydroxide nanocomposite structures prepared in Example 2.

[0023] Figure 5 This is the morphology of the conical and hexagonal layered cobalt hydroxide nanocomposite structure prepared in Example 3.

[0024] Figure 6 This is the morphology of the conical and hexagonal layered cobalt hydroxide nanocomposite structure prepared in Example 4.

[0025] Figure 7 This is the morphology of the conical and hexagonal layered cobalt hydroxide nanocomposite structure prepared in Example 5. DETAILED DESCRIPTION

[0026] The following is a detailed description of the embodiments of the present invention. The embodiments of the present invention are not limited to the embodiments described in the embodiments. The present invention uses cyclic voltammetry for electrochemical control, as follows: Working electrode 1*1cm 2 , the counter electrode is a platinum sheet 1*1cm 2 , the reference electrode is Hg / HgO electrode.

[0027] Example 1

[0028] S1 Preparation of vanadium-doped cobalt hydroxide: Vanadium-doped cobalt hydroxide was grown by hydrothermal method using nickel foam as a substrate, wherein the concentration of cobalt chloride was 0.5 mol / L, the concentration of vanadium trichloride was 0.2 mol / L, the concentration of urea was 0.8 mol / L, the concentration of ammonium fluoride was 0.2 mol / L, the solution pH was 9.6, the hydrothermal temperature was 110°C, and the reaction time was 8 h.

[0029] S2 Preparation of vanadium-doped cobalt oxide: The vanadium-doped cobalt hydroxide sample prepared in S1 was annealed in a tube furnace, the annealing temperature was set to 200°C, the insulation time was 3h, and a vanadium-doped cobalt oxide sample was prepared.

[0030] S3 electrochemical reconstruction of cobalt hydroxide: The vanadium-doped cobalt oxide sample prepared in S2 was used as the working electrode, the electrolyte was 2 mol / L KOH solution, and the cyclic voltammetry method was used with a scanning speed of 2 mV / s. After repeating the scanning for 5 times, the conical and hexagonal layered cobalt hydroxide nanocomposite structures described in the present invention were obtained.

[0031] The morphology of the vanadium-doped cobalt hydroxide prepared in step S1 is as follows: Figure 1 As shown. Figure 1 It can be seen that the vanadium-doped cobalt hydroxide cone structure has a smooth surface, a thin top and a thick bottom, and a thin sheet structure is interspersed in the cone structure, and the thickness of the thin sheet is 46 nm.

[0032] The XRD pattern of the cobalt hydroxide nanocomposite structure obtained in step S3 is as follows: Figure 2 As shown in the figure, after comparison, it is basically consistent with the Co(OH)2 standard spectrum (PDF:51-1731), which proves that the component of the composite structure is cobalt hydroxide. Figure 3 As shown, the thickness of the hexagonal layered structure is 157nm.

[0033] Example 2

[0034] S1 Preparation of vanadium-doped cobalt hydroxide: Vanadium-doped cobalt hydroxide was grown by hydrothermal method using nickel foam as a substrate, wherein the concentration of cobalt nitrate was 0.3 mol / L, the concentration of vanadium sulfate was 0.1 mol / L, the concentration of urea was 0.5 mol / L, the concentration of ammonium fluoride was 0.1 mol / L, the solution pH was 8.5, the hydrothermal temperature was 120°C, and the reaction time was 10 h.

[0035] S2 Preparation of vanadium-doped cobalt oxide: The vanadium-doped cobalt hydroxide sample prepared in S1 was annealed in a tube furnace, the annealing temperature was set to 250° C., the insulation time was 5 h, and a vanadium-doped cobalt oxide sample was prepared.

[0036] S3 electrochemical reconstruction of cobalt hydroxide: The vanadium-doped cobalt oxide sample prepared in S2 was used as the working electrode, the electrolyte was 5 mol / L KOH solution, and the cyclic voltammetry method was used with a scanning speed of 5 mV / s. After repeating the scanning for 20 times, the conical and hexagonal layered cobalt hydroxide nanocomposite structures described in the present invention were obtained.

[0037] The morphology of the cobalt hydroxide nanocomposite structure obtained in step S3 is shown in FIG. Figure 4 (a) and Figure 4 As shown in (b), Figure 4 (a) It can be clearly seen that the cone-shaped structure in the composite structure is thin at the top and thick at the bottom. Figure 4 The thickness of the hexagonal layered structure in (b) is 233 nm.

[0038] Example 3

[0039] S1 Preparation of vanadium-doped cobalt hydroxide: Vanadium-doped cobalt hydroxide was grown by hydrothermal method using nickel foam as a substrate, wherein the concentration of cobalt sulfate was 0.5 mol / L, the concentration of vanadium trichloride was 0.1 mol / L, the concentration of urea was 0.6 mol / L, the concentration of ammonium fluoride was 0.2 mol / L, the solution pH was 8.7, the hydrothermal temperature was 130°C, and the reaction time was 24 h.

[0040] S2 Preparation of vanadium-doped cobalt oxide: The vanadium-doped cobalt hydroxide sample prepared in S1 was annealed in a tube furnace, the annealing temperature was set to 400°C, the insulation time was 3h, and a vanadium-doped cobalt oxide sample was prepared.

[0041] S3 electrochemical reconstruction of cobalt hydroxide: The vanadium-doped cobalt oxide sample prepared in S2 was used as the working electrode, the electrolyte was 3 mol / L KOH solution, and the cyclic voltammetry method was used with a scanning speed of 3 mV / s. After repeating the scanning for 150 times, the conical and hexagonal layered cobalt hydroxide nanocomposite structures described in the present invention were obtained.

[0042] The morphology of the cobalt hydroxide nanocomposite structure obtained in step S3 is shown in FIG. Figure 5 As shown, the thickness of the hexagonal layered structure is 236nm.

[0043] Example 4

[0044] S1 Preparation of vanadium-doped cobalt hydroxide: Vanadium-doped cobalt hydroxide was grown by hydrothermal method using nickel foam as a substrate, wherein the concentration of cobalt chloride was 0.3 mol / L, the concentration of vanadium sulfate was 0.1 mol / L, the concentration of urea was 0.4 mol / L, the concentration of ammonium fluoride was 0.1 mol / L, the solution pH was 8.3, the hydrothermal temperature was 130°C, and the reaction time was 12 h.

[0045] S2 Preparation of vanadium-doped cobalt oxide: The vanadium-doped cobalt hydroxide sample prepared in S1 was annealed in a tube furnace, the annealing temperature was set to 280° C., the insulation time was 8 h, and a vanadium-doped cobalt oxide sample was prepared.

[0046] S3 electrochemical preparation of cobalt hydroxide: The vanadium-doped cobalt oxide sample prepared in S2 was used as the working electrode, the electrolyte was a 5 mol / L KOH solution, and the cyclic voltammetry method was used with a scanning speed of 7 mV / s. After repeating the scanning for 300 times, the conical and hexagonal layered cobalt hydroxide nanocomposite structures described in the present invention were obtained.

[0047] The morphology of the cobalt hydroxide nanocomposite structure obtained in step S3 is shown in FIG. Figure 6 As shown, the thickness of the hexagonal layered structure is 302nm.

[0048] Example 5

[0049] S1 Preparation of vanadium-doped cobalt hydroxide: Vanadium-doped cobalt hydroxide was grown by hydrothermal method using nickel foam as a substrate, wherein the concentration of cobalt nitrate was 0.8 mol / L, the concentration of vanadium trichloride was 0.2 mol / L, the concentration of urea was 0.5 mol / L, the concentration of ammonium fluoride was 0.2 mol / L, the solution pH was 8.5, the hydrothermal temperature was 120°C, and the reaction time was 9 h.

[0050] S2 Preparation of vanadium-doped cobalt oxide: The vanadium-doped cobalt hydroxide sample prepared in S1 was annealed in a tube furnace, the annealing temperature was set to 330° C., the insulation time was 6 h, and a vanadium-doped cobalt oxide sample was prepared.

[0051] S3 electrochemical reconstruction of cobalt hydroxide: The vanadium-doped cobalt oxide sample prepared in S2 was used as the working electrode, the electrolyte was 4 mol / L KOH solution, and the cyclic voltammetry method was used with a scanning speed of 3.5 mV / s. After repeating the scanning for 85 times, the conical and hexagonal layered cobalt hydroxide nanocomposite structures described in the present invention were obtained.

[0052] The morphology of the cobalt hydroxide nanocomposite structure obtained in step S3 is shown in FIG. Figure 7 As shown, the thickness of the hexagonal layered structure is 820nm.

[0053] from Figures 3 to 7It can be seen that the structure of cobalt hydroxide after electrochemical reconstruction and regulation is significantly different from the structure of vanadium-doped cobalt hydroxide prepared by hydrothermal reaction. The specific change is that the original smooth conical structure will produce a rough surface, and the original smooth thin sheet structure surface becomes rough and becomes a thicker hexagonal structure, and the hexagonal sheet structure is composed of several thin sheet layers stacked. Therefore, the electrochemical reconstruction and regulation of the present invention can induce the original smooth conical structure and lamellar structure to be transformed into a rough surface conical structure and a rough surface and a thick hexagonal structure stacked by several thin sheets. This obvious structural transformation can significantly improve its specific capacitance, that is, significantly improve the electrochemical performance.

[0054] The specific capacitance test was performed on the vanadium-doped cobalt hydroxide prepared in step S1 of Examples 1-5 and the cobalt hydroxide composite structure prepared in step S3, respectively. The specific test method is as follows:

[0055] The test results are shown in Table 1. Table 1 lists the specific capacitance data calculated based on the discharge time at a current density of 1A / g using a three-electrode system after constant current charge and discharge tests. By comparison, it can be seen that the specific capacitance of the cobalt hydroxide composite structure prepared by S3 electrochemical reconstruction regulation is higher than that of S1 vanadium-doped cobalt hydroxide, which proves that the cobalt hydroxide with rough surface cone and hexagonal layered composite structure prepared by electrochemical reconstruction has better electrochemical performance.

[0056] Table 1 Specific capacitance test values ​​of vanadium-doped cobalt hydroxide and cobalt hydroxide nanocomposite structures

[0057] Example 1 Example 2 Example 3 Example 4 Example 5 Vanadium-doped cobalt hydroxide 879F / g 812F / g 905F / g 793F / g 766F / g Cobalt hydroxide composite structure 1435F / g 1510F / g 1612F / g 1509F / g 1421F / g .

Claims

1. A conical and hexagonal layered cobalt hydroxide nanocomposite structure, characterized in that: The cobalt hydroxide nanocomposite structure is composed of a cone structure and a layered structure; the cone structure is thin at the top, thick at the bottom and has a rough surface; the layered structure has a rough surface and a layered structure, and is formed by stacking a number of thin sheets.

2. The conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 1, characterized in that: The layered structure has a thickness of 150 nm to 820 nm.

3. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 1 or 2, characterized in that: The following steps are involved: S1 preparation of vanadium-doped cobalt hydroxide: using a weak alkaline solution containing cobalt ions, vanadium ions and a precipitant as a raw material, synthesizing vanadium-doped cobalt hydroxide on a foamed nickel substrate through a hydrothermal reaction; S2: Preparation of vanadium-doped cobalt oxide: thermally annealing the vanadium-doped cobalt hydroxide prepared in S1 to obtain foamed nickel / vanadium-doped cobalt oxide; S3 electrochemical reconstruction of cobalt hydroxide: The nickel foam / vanadium-doped cobalt tetroxide prepared in S2 is used as the working electrode, and electrochemical scanning is repeated in a potassium hydroxide solution. Under the electrochemical action, the doped vanadium dissolves in the alkaline solution to induce surface reconstruction of the material, thereby obtaining the conical and hexagonal layered cobalt hydroxide nanocomposite structure.

4. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 3, characterized in that: The electrochemical scan in step S3 includes cyclic voltammetry, with a scan rate of 1 to 8 mV / s and a number of repeated scans of 5 to 300 cycles; the concentration of the potassium hydroxide solution is 1 to 6 mol / L.

5. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 3, characterized in that: In step S1, the molar ratio of cobalt ions to vanadium ions is V / Co<0.

5.

6. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 3, characterized in that: In step S1, the cobalt ions are from strong acid salts of cobalt, including one of cobalt nitrate, cobalt chloride and cobalt sulfate; the vanadium ions are from one of vanadium chloride and vanadium sulfate; and the precipitant includes urea and ammonium fluoride.

7. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 3, characterized in that: The hydrothermal reaction temperature in step S1 is 110-130° C., and the reaction time is 8-24 hours; the pH of the weak alkaline solution is 8-12.

8. The method for preparing the conical and hexagonal layered cobalt hydroxide nanocomposite structure according to claim 3, characterized in that: The annealing treatment in step S2 is performed at a temperature of 200 to 400° C. and for a treatment time of 3 to 10 hours.