Preparation of three-dimensional flower-shaped NiWO4 / WO3 composite material and application of composite material in gas sensor
The preparation of three-dimensional flower-like NiWO4/WO3 composite materials through solvent and hydrothermal heat solves the problem of insufficient response and stability of the sensor at low temperatures, and realizes efficient detection of trimethylamine, with fast response, excellent selectivity and long-term stability , suitable for applications in the field of food monitoring.
Patent Information
- Application Number
- CN202410873958.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-12
AI Technical Summary
Existing metal oxide semiconductor sensors lack sensing response, selectivity and stability at low temperatures, especially when detecting trimethylamine gas, it is difficult to meet the needs of food safety and health monitoring.
Through the technology of combining solvent heat and hydrothermal heat, a three-dimensional flower-like NiWO4/WO3 composite material is prepared to improve the response, selectivity and stability of the sensor and apply it to the detection of trimethylamine.
It realizes the ability to effectively detect trimethylamine at low temperatures, has fast response and recovery time, excellent selectivity and long-term stability, is suitable for large-scale industrial production, and is suitable for food monitoring.
Smart Images

Figure CN118929781A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation and application of a composite material, in particular to the preparation of a three-dimensional flower-shaped NiWO4 / WO3 composite material and the application of the composite material in a gas sensor. Background Art
[0002] Trimethylamine (TMA) is a volatile organic compound commonly found in seafood, biological specimens, and industrial environments. TMA is associated with the process of food spoilage and degradation, and highly spoiled seafood will release large amounts of TMA, which can produce a foul odor. To assess the freshness of seafood, TMA concentration is considered a reliable indicator, with levels below 10 ppm indicating freshness, 10-50 ppm indicating initial decay, and more than 60 ppm indicating deep decay, emphasizing the importance of its detection in ensuring food safety and quality control. In addition, TMA is considered an important biomarker for disease diagnosis and human health monitoring. For example, individuals with chronic kidney disease have exhaled TMA concentrations exceeding 0.2 ppm, indicating its potential utility as a biomarker for chronic kidney disease monitoring. Therefore, the detection and quantification of TMA levels have become key in environmental monitoring, ensuring food safety, and medical diagnosis.
[0003] Gas detection devices such as semiconductor sensors, fiber optic sensors, and mass sensors have made great progress and have been widely used in environmental monitoring, industrial safety, healthcare, and other fields. With the development of the Internet of Things, sensors have become a key facilitator for enhancing personal safety and environmental sustainability. Among them, metal oxide semiconductor sensors, known for their high sensitivity, straightforward manufacturing, cost efficiency, and seamless integration with modern control systems, have attracted considerable interest. It is worth noting that tungsten trioxide (WO3), as a typical n-type semiconductor, has been widely studied due to its special physical and chemical properties and has shown great potential in detecting oxidizing and reducing gases. However, further improvements are needed to optimize the sensing response, selectivity, stability, and response / recovery time of WO3 sensors at low temperatures. Given that the gas sensing process in metal oxide sensors is mainly controlled by solid-gas interface reactions, creating unique structures or interfaces can greatly improve the performance of sensors. Advances in nanotechnology have significantly enhanced the functionality of metal oxide sensors due to their considerable surface-to-volume ratio and unique magnetic, optical, and electrical properties. Of particular note are three-dimensional (3D) hierarchical micro-nanostructures, which are characterized by a large number of active sites and rich pore structures, which facilitate gas diffusion and molecular adsorption, resulting in excellent gas sensing capabilities. In addition, creating pn or nn heterojunctions to regulate the surface interface is an effective strategy to enhance the gas-sensing properties. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method of a three-dimensional flower-shaped NiWO4 / WO3 composite material and its application in a gas sensor. The present invention designs and synthesizes a NiWO4-functionalized three-dimensional WO3 flower-shaped structure sensitive material by combining solvent thermal and hydrothermal technology, which is applied to the detection of trimethylamine and has good response, significant selectivity and excellent long-term stability.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A three-dimensional flower-shaped NiWO4 / WO3 composite material is prepared, including the following preparation process:
[0007] (1) Dissolve 2.5 g of H2WO4 in a solution containing 50 mL of deionized water and 34 mL of H2O2, heat to 95°C in a water bath, and stir until the solution becomes clear; then, add deionized water to dilute the solution to 200 mL to form a WO3 precursor solution;
[0008] (2) Add 60 mL of acetonitrile (CH3CN) and 5 mL of hydrochloric acid (HCl, 3M) to 15 mL of WO3 precursor solution; then add 0.1 g of oxalic acid and 0.1 g of urea, and stir magnetically until completely dissolved; transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 180°C for 2 h; after cooling naturally to room temperature, collect the resulting precipitate, wash it alternately with deionized water and ethanol three times, and then dry it at 60°C overnight. Finally, the product was calcined in a muffle furnace at 500°C for 2 h to obtain a flower-like structure WO3 material;
[0009] (3) The prepared flower-structured WO3 material (0.108 g) was dispersed in 40 mL of deionized water and ultrasonicated at room temperature for 30 min. Subsequently, a certain amount of nickel nitrate hexahydrate (Ni(NO3)2·6H2O) and sodium tungstate dihydrate (Na2WO4·2H2O) were added to the WO3 suspension and magnetically stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and kept at 200°C for 5 h. After naturally cooling to room temperature, the precipitate was collected by centrifugation, washed repeatedly with deionized water and ethanol, and then dried at 60°C for 12 h.
[0010] (4) The dried product was placed in a clean crucible in a muffle furnace and calcined at 500° C. for 2 h to obtain a flower-like NiWO4 / WO3 composite material, which was stored in a desiccator for analysis and testing.
[0011] A three-dimensional flower-shaped NiWO4 / WO3 composite material is used in a gas sensor. The material is used as a gas sensitive material to make a gas sensor for detecting trimethylamine gas, and the steps are as follows:
[0012] NiWO4 / WO3 and pure WO3 powders were ground and mixed with ethanol to make a uniform slurry; this slurry was then applied as a coating on the outer surface of a ceramic tube, whose electrodes consisted of four platinum wires and two gold electrodes spaced 6nm apart; a Ni-Cr heating wire passed through the ceramic tube as the ethanol evaporated to form a sensing film; subsequently, the Ni-Cr heating wire and the Pt wire were welded to a hexagonal base to assemble the gas sensor; finally, the gas sensor was placed on a WS-30A and aged at 400°C for 48h to ensure stability.
[0013] The advantages and effects of the present invention are:
[0014] (1) The NiWO4 / WO3 trimethylamine sensor prepared by the present invention effectively reduces the operating temperature;
[0015] (2) The sensor prepared by the present invention has a relatively fast response and recovery time, as well as excellent selectivity and long-term stability;
[0016] (3) The NiWO4 / WO3 trimethylamine sensor prepared by the present invention has a simple preparation method, is easy to assemble, is suitable for large-scale industrial production, and has broad application prospects in the field of food monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 XRD patterns of materials obtained for Examples 1-5;
[0018] Figure 2 FE-SEM images of the materials obtained in Examples 1-5, (a)-(b) WO3; (c)-(d) 5-NiWO4 / WO3; (e)-(f) 10-NiWO4 / WO3; (g)-(h) 15-NiWO4 / WO3; (i)-(j) 20-NiWO4 / WO3;
[0019] Figure 3 Schematic diagram of the structure of the trimethylamine sensor;
[0020] Figure 4 It is the sensitivity of the gas sensor to 10ppm trimethylamine gas at a test temperature of 50-350℃;
[0021] Figure 5 The relationship between the response of the gas sensor at 150°C and the concentration of trimethylamine (0.1-100 ppm);
[0022] Figure 6 The selectivity of the gas sensor to various gases at 10ppm at 150℃;
[0023] Figure 7The gas sensor of Example 3 is (a) the response-recovery curve of trimethylamine gas of different concentrations at 150°C, (b) the response-recovery curve of 10 ppm trimethylamine gas, (c) the repeatability curve of 10 ppm trimethylamine gas, and (d) the response of the gas sensor to trimethylamine of different concentrations within 30 days;
[0024] Figure 8 This is a product diagram of the embodiment. DETAILED DESCRIPTION
[0025] The present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings.
[0026] A method for preparing a three-dimensional flower-shaped NiWO4 / WO3 composite material comprises the following steps:
[0027] Example 1
[0028] Preparation of three-dimensional flower-shaped WO3
[0029] Step 1: Dissolve 2.5 g of H2WO4 in a solution containing 50 mL of deionized water and 34 mL of H2O2, heat to 95 °C in a water bath, and stir until the solution becomes clear. Subsequently, add deionized water to dilute the solution to 200 mL to form a WO3 precursor solution;
[0030] Step 2: Add 60 mL of CH3CN and 5 mL of HCl (3M) to 15 mL of WO3 precursor solution. Then add 0.1 g of oxalic acid and 0.1 g of urea and stir magnetically until completely dissolved. Transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 180 °C for 2 h.
[0031] Step 3: The powder collected in step 2 is washed by centrifugation with deionized water and ethanol for three times, and then dried at 60°C for later use;
[0032] Step 4: Place the precursor prepared in step 3 directly into a muffle furnace and heat it to 500°C and keep it for 2 hours to obtain pure WO3 flower.
[0033] Example 2
[0034] Preparation of three-dimensional flower-like 5-NiWO4 / WO3 composite materials
[0035] Steps 1, 2, 3 and 4 are the same as in Example 1;
[0036] Step 5: Disperse 0.1080 g of the prepared WO3 flower in 40 mL of deionized water and ultrasonicate for 30 min at room temperature. Then, add 0.0068 g of Ni(NO3)2·6H2O and 0.0077 g of Na2WO4·2H2O to the WO3 suspension and stir magnetically for 30 min. Transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 200 °C for 5 h.
[0037] Step 6: The powder collected in step 5 is washed by centrifugation with deionized water and ethanol three times respectively, and then dried at 60°C for later use;
[0038] Step 7: Place the dried product of step 6 into a clean crucible and place it in a muffle furnace, calcine at 500° C. for 2 h to obtain a flower-shaped 5-NiWO4 / WO3 composite material, which is stored in a desiccator for analysis and testing.
[0039] Example 3
[0040] Preparation of three-dimensional flower-shaped 10-NiWO4 / WO3 composites
[0041] Steps 1, 2, 3 and 4 are the same as in Example 1;
[0042] Step 5: Disperse 0.1080 g of the prepared WO3 flower in 40 mL of deionized water and ultrasonicate for 30 min at room temperature. Then, add 0.0135 g of Ni(NO3)2·6H2O and 0.0154 g of Na2WO4·2H2O to the WO3 suspension, stir magnetically for 30 min, and transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 200 °C for 5 h.
[0043] Steps 6 and 7 are the same as in Example 2.
[0044] Example 4
[0045] Preparation of three-dimensional flower-shaped 15-NiWO4 / WO3 composites
[0046] Steps 1, 2, 3 and 4 are the same as in Example 1
[0047] Step 5: Disperse 0.1080 g of the prepared WO3 flower in 40 mL of deionized water and ultrasonicate for 30 min at room temperature. Then, add 0.0203 g of Ni(NO3)2·6H2O and 0.0230 g of Na2WO4·2H2O to the WO3 suspension and stir magnetically for 30 min. Transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 200 °C for 5 h.
[0048] Steps 6 and 7 are the same as in Example 2.
[0049] Example 5
[0050] Preparation of three-dimensional flower-like 20-NiWO4 / WO3 composite materials
[0051] Steps 1, 2, 3 and 4 are the same as in Example 1
[0052] Step 5: Disperse 0.1080 g of the prepared WO3 flower in 40 mL of deionized water and ultrasonicate for 30 min at room temperature. Then, add 0.0271 g of Ni(NO3)2·6H2O and 0.0307 g of Na2WO4·2H2O to the WO3 suspension and stir magnetically for 30 min. Transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 200 °C for 5 h.
[0053] Steps 6 and 7 are the same as in Example 2.
[0054] Structural characterization of NiWO4 / WO3 composites
[0055] (1) XRD analysis
[0056] The XRD spectra of the materials obtained in Example 1-5 are as follows Figure 1 As shown. WO3 has good crystallinity, corresponding to the orthorhombic phase WO3 (JPCDS43-1035). The diffraction peaks of the NiWO4 / WO3 composite material are all arranged in the same way as the diffraction peaks of WO3, indicating that the incorporation of NiWO4 does not significantly change the phase composition. It is worth noting that the XRD spectra of Example 2 and Example 3 do not show obvious NiWO4 peaks, which may be due to the low concentration of NiWO4 in these composite materials and the limited diffraction intensity. As the NiWO4 content increases, Example 4 shows obvious NiWO4 diffraction peaks, and as the NiWO4 content increases, the diffraction peaks gradually increase. These peaks correspond to NiWO4 (JPCDSNo.150755), confirming the successful preparation of the NiWO4 / WO3 composite material. All samples show sharp diffraction peaks, indicating that the product has good crystallinity and high purity.
[0057] (2) SEM analysis
[0058] The scanning electron microscope microstructure of the materials obtained in Examples 1-5 was analyzed. Figure 2As shown, the pure WO3 product has a clear flower-like structure with relatively uniform size and random distribution. Ultrathin nanosheets with diameters ranging from 6 to 11 μm and thicknesses of about 10 to 30 nm are intertwined to form a multilayer structure. This unique structure provides ample voids and a large surface area, significantly improving the sensing performance. It is worth noting that even with the addition of different amounts of NiWO4, the NiWO4 / WO3 composite material still maintains a flower-like structure. In addition, the surface of the NiWO4 / WO3 composite material becomes significantly rough, and nanoparticles are attached to the surface of the nanosheets. With the increase of NiWO4 content, the size of the NiWO4 nanoparticles gradually increases and becomes more heterogeneous, resulting in the destruction of some WO3 micro-nanoflowers.
[0059] Gas Sensing Performance Test of NiWO4 / WO3 Composite Material
[0060] The NiWO4 / WO3 composite material is added to anhydrous ethanol to form a uniform slurry, which is then coated on an Al2O3 ceramic tube. The Al2O3 ceramic tube has two gold electrodes and four platinum wires, and a nickel-chromium heating wire in the tube. The ceramic tube is welded on a six-legged base, such as Figure 3 As shown, a gas sensor element is manufactured. Figure 4 The sensor response to 10 ppm trimethylamine at different operating temperatures is shown in Figure 2. The response of all the sensors in the examples initially increases with the increase of the operating temperature until it reaches a maximum value, and then decreases with the continued increase of the temperature, thus presenting an "increase-maximum-decline" pattern. It is worth noting that the addition of NiWO4 is conducive to lowering the optimal operating temperature and improving the sensor response in a lower temperature range, thereby enhancing the reliability and stability of practical applications. Among all the sensors, the sensor in Example 3 exhibits the highest trimethylamine sensor response (12.06 / 150°C). Figure 5 The sensing response to different concentrations of trimethylamine at 150°C is shown. As the concentration of trimethylamine (1-20ppm) increases, the response of all sensors increases rapidly. Subsequently, when the concentration of trimethylamine increases further, this upward trend gradually slows down, which may be due to the adsorption saturation of high-concentration trimethylamine. In addition, it is worth noting that at each trimethylamine concentration, the sensor of Example 3 always shows the highest response and is able to detect trimethylamine as low as 0.1ppm (the response is about 1.38), further demonstrating the sensitization effect of the NiWO4 functionalized WO3 flower-like structure. Figure 6 The figure shows the selectivity test of the sensor to various gases at 10 ppm. It can be seen that the response of the sensor to other interfering gases (ethanol, methanol, formaldehyde, acetone and ammonia) is negligible, indicating that the sensor has good selectivity to trimethylamine. Figure 7(a) shows the response / recovery behavior of the sensor of Example 3 at different trimethylamine concentrations. Even at low concentrations (0.1 ppm), the resistance recovers to the baseline level after each trimethylamine removal cycle. The sensor has stable and repeatable sensing characteristics, indicating that it is suitable for detecting trimethylamine gas over a wide concentration range. Figure 7 (b) shows the dynamic response / recovery characteristics of the sensor of Example 3 to 10 ppm trimethylamine at 150°C. After the introduction of trimethylamine, the resistance of the sensor of Example 3 continued to decrease, indicating a typical n-type sensing behavior. The response / recovery times were 14 / 17 s, respectively, indicating that the sensor of Example 3 had good response / recovery characteristics. Figure 7 (c) shows that at an operating temperature of 150°C, Example 3 shows a consistent adsorption-desorption pattern for five cycles of 10 ppm trimethylamine in each cycle, and the resistance of the sensor always returns to the initial value, showing excellent repeatability. Figure 7 (d) It can be seen that over the course of 30 days, the response values of the sensor of Example 3 to various trimethylamine concentrations (0.1 ppm, 1 ppm, 5 ppm and 10 ppm) did not change, indicating that it has good long-term stability.
Claims
1. Preparation of a three-dimensional flower-shaped NiWO4 / WO3 composite material, characterized in that: The preparation process includes the following: (1) Dissolve 2.5 g of H2WO4 in a solution containing 50 mL of deionized water and 34 mL of H2O2, heat to 95°C in a water bath, and stir until the solution becomes clear; then, add deionized water to dilute the solution to 200 mL to form a WO3 precursor solution; (2) Add 60 mL of acetonitrile (CH3CN) and 5 mL of hydrochloric acid (HCl, 3M) to 15 mL of WO3 precursor solution; then add 0.1 g of oxalic acid and 0.1 g of urea, and stir magnetically until completely dissolved; transfer the resulting solution to a stainless steel autoclave lined with polytetrafluoroethylene and react at 180°C for 2 h; after cooling naturally to room temperature, collect the resulting precipitate, wash it alternately with deionized water and ethanol three times, and then dry it at 60°C overnight. Finally, the product was calcined in a muffle furnace at 500°C for 2 h to obtain a flower-like structure WO3 material; (3) The prepared flower-structured WO3 material (0.108 g) was dispersed in 40 mL of deionized water and ultrasonicated at room temperature for 30 min. Subsequently, a certain amount of nickel nitrate hexahydrate (Ni(NO3)2·6H2O) and sodium tungstate dihydrate (Na2WO4·2H2O) were added to the WO3 suspension and magnetically stirred for 30 min. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and kept at 200°C for 5 h. After naturally cooling to room temperature, the precipitate was collected by centrifugation, washed repeatedly with deionized water and ethanol, and then dried at 60°C for 12 h. (4) The dried product was placed in a clean crucible in a muffle furnace and calcined at 500° C. for 2 h to obtain a flower-like NiWO4 / WO3 composite material, which was stored in a desiccator for analysis and testing.
2. A three-dimensional flower-shaped NiWO4 / WO3 composite material is used in gas sensors, characterized in that: The material is used as a gas sensitive material to make a gas sensor for detecting trimethylamine gas, and the steps are as follows: NiWO4 / WO3 and pure WO3 powders were ground and mixed with ethanol to make a uniform slurry; this slurry was then applied as a coating on the outer surface of a ceramic tube, whose electrodes consisted of four platinum wires and two gold electrodes spaced 6nm apart; a Ni-Cr heating wire passed through the ceramic tube as the ethanol evaporated to form a sensing film; subsequently, the Ni-Cr heating wire and the Pt wire were welded to a hexagonal base to assemble the gas sensor; finally, the gas sensor was placed on a WS-30A and aged at 400°C for 48h to ensure stability.